FeCu / ZSM-5 catalyst, preparation method thereof and application of FeCu / ZSM-5 catalyst in preparation of acetic acid by catalyzing methane carbonylation reaction
By introducing Cu species into Fe/ZSM-5 catalyst, the FeCu/ZSM-5 catalyst was prepared, which inhibited the coupling of hydroxyl and methyl radicals, and solved the problem of low selectivity of existing catalysts for acetic acid, achieving the highest 70.1% acetic acid selectivity and side reaction inhibition effect.
Patent Information
- Application Number
- CN202411113165.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Fe/ZSM-5 catalysts have low selectivity for acetic acid in methane carbonylation reaction, up to 63.2%, and the formation of C1 and C2 products is a competitive reaction, making it difficult to effectively improve the output selectivity of acetic acid.
The Cu species were introduced on the basis of the Fe/ZSM-5 catalyst. The FeCu/ZSM-5 catalyst was prepared by vacuum impregnation, rotary evaporation and calcination with ammonium-type ZSM-5 molecular sieve. The Cu species inhibited the The coupling of hydroxyl and methyl radicals increases the selectivity of acetic acid.
The selectivity of acetic acid was improved to up to 70.1%, and the occurrence of side reactions was inhibited and the performance of the catalyst was improved.
Smart Images

Figure CN119016095A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalytic technology, in particular to a FeCu / ZSM-5 material and a preparation method thereof, and application thereof in catalyzing methane carbonylation reaction to produce acetic acid. Background Art
[0002] Acetic acid is a bulk chemical product and one of the most important organic acids. It can be used to produce vinyl acetate, acetic anhydride, acetate and cellulose acetate. Direct carbonylation of methane to produce acetic acid is considered to be the most promising route for the production of acetic acid in the future. Zeolite-supported metal catalysts, especially Fe / ZSM-5, have been widely studied for the carbonylation of methane to produce acetic acid.
[0003] The inventors previously prepared Fe / ZSM-5 catalysts containing mononuclear Fe sites by impregnation method, which effectively promoted the production of acetic acid (Wang, C.-W.; Sun, Y.; Wang, L.-J.; Feng, W.-H.; Miao, Y.-T.; Yu, M.-M.; Wang, Y.-X.; Gao, X.-D.; Zhao, Q.; Ding, Z.; Feng, Z.; Yu, S.-M.; Yang, J.; Hu, Y.; Wu, J.-F., Appl. Catal., B 2023, 329, 122549). However, the selectivity of the above catalysts for acetic acid is not high, with the highest value being 63.2%. Summary of the invention
[0004] The object of the present invention is to provide a FeCu / ZSM-5 catalyst and a preparation method thereof and application thereof in catalyzing the carbonylation reaction of methane to produce acetic acid. The FeCu / ZSM-5 catalyst provided by the present invention is applied to the carbonylation reaction of methane to produce acetic acid and has high selectivity for the target product acetic acid.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a FeCu / ZSM-5 catalyst, comprising a ZSM-5 molecular sieve and an active component loaded on the ZSM-5 molecular sieve;
[0007] The active components include Fe species and Cu species; the Fe species include mononuclear Fe, oligomeric Fe and nano Fe2O3 particles; the Cu species include mononuclear Cu;
[0008] The content of Fe element in the FeCu / ZSM-5 catalyst is 0.4-0.6 wt %, and the content of Cu element is 0.1-0.25 wt %.
[0009] The preparation method of the FeCu / ZSM-5 catalyst comprises the following steps: dissolving an iron salt and a copper salt into water to obtain a metal salt solution;
[0010] The ammonium ZSM-5 molecular sieve is mixed with the metal salt solution for vacuum impregnation, and the obtained impregnation liquid is rotary evaporated and dried to obtain a FeCu / ZSM-5 catalyst precursor; the masses of the Fe element and the Cu element in the metal salt solution are respectively equal to the masses of the Fe element and the Cu element in the target FeCu / ZSM-5 catalyst;
[0011] The FeCu / ZSM-5 catalyst precursor is calcined under static air to obtain the FeCu / ZSM-5 catalyst.
[0012] Preferably, the calcination temperature is 500° C., and 500° C. is maintained for 3 hours.
[0013] Preferably, the vacuum impregnation comprises: firstly subjecting the ammonium ZSM-5 molecular sieve to a first vacuum treatment under closed conditions, then injecting a metal salt solution to continue a second vacuum treatment, and finally stirring at room temperature.
[0014] Preferably, the first vacuum treatment lasts for 20 to 40 minutes, and the vacuum degree is 0.05 to 0.1 MPa.
[0015] Preferably, the second vacuum treatment lasts for 5 to 20 minutes, and the vacuum degree is 0.05 to 0.1 MPa.
[0016] Preferably, the stirring time is 20 to 28 hours, and the stirring rate is 700 to 900 rpm.
[0017] Preferably, the temperature of the rotary evaporation is 65-75°C; the temperature of the drying is 70-90°C.
[0018] Preferably, the ammonium-type ZSM-5 molecular sieve is a Na-type ZSM-5 molecular sieve obtained by ammonium ion exchange.
[0019] The present invention provides the use of the FeCu / ZSM-5 catalyst described in the above scheme or the FeCu / ZSM-5 catalyst prepared by the preparation method described in the above scheme in catalyzing methane carbonylation reaction to produce acetic acid.
[0020] The present invention provides a FeCu / ZSM-5 catalyst, comprising a ZSM-5 molecular sieve and an active component loaded on the ZSM-5 molecular sieve; the active component comprises an Fe species and a Cu species; the Fe species comprises mononuclear Fe, oligomeric Fe and nano Fe2O3 particles; the Cu species comprises mononuclear Cu; the content of Fe element in the FeCu / ZSM-5 catalyst is 0.4-0.6wt%, and the content of Cu element is 0.1-0.25wt%. The products of methane oxidative carbonylation include C1 products (mainly methanol and formic acid, formic acid is mainly produced by oxidation of methanol) and C2 products (acetic acid), and the generation of C1 and C2 products is a competitive reaction. The present invention adds a Cu species on the basis of the Fe / ZSM-5 catalyst, and the addition of the Cu species inhibits the coupling of hydroxyl radicals and methyl radicals, thereby improving the selectivity of acetic acid. The results of the embodiment show that the FeCu / ZSM-5 catalyst provided by the present invention has a selectivity of up to 70.1% for acetic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a temperature program diagram for calcining ZSM-5 molecular sieve raw powder to remove the template;
[0022] Figure 2 PXRD patterns of the catalysts prepared in Comparative Example 1 and Comparative Examples 3 to 6;
[0023] Figure 3 Cu 0.5 / UV-visible absorption spectrum of ZSM-5;
[0024] Figure 4 The catalytic performance diagram of (FeCu) / ZSM-5 catalysts with different Cu loadings;
[0025] Figure 5 This is the experimental evidence for the free radical mechanism of spin trapping in the methane carbonylation reaction catalyzed by (FeCu) / ZSM-5 catalyst. DETAILED DESCRIPTION
[0026] The present invention provides a FeCu / ZSM-5 catalyst, comprising a ZSM-5 molecular sieve and an active component loaded on the ZSM-5 molecular sieve;
[0027] The active components include Fe species and Cu species; the Fe species include mononuclear Fe, oligomeric Fe and nano Fe2O3 particles; the Cu species include mononuclear Cu, preferably tetrahedral mononuclear Cu and octahedral mononuclear Cu;
[0028] The Fe content of the FeCu / ZSM-5 catalyst is 0.4-0.6wt%, preferably 0.5wt%; the Cu content is 0.1-0.25wt%, specifically 0.1wt%, 0.15wt%, 0.2wt% or 0.25wt%, which will not be enumerated here.
[0029] In the present invention, the mononuclear Fe, oligomeric Fe and mononuclear Cu are well-known concepts in the art. Among them, mononuclear Fe emphasizes that the active center has only one Fe atom, and there are other coordinated atoms around it, which are generally the framework oxygen, hydroxyl and water of the molecular sieve; oligomeric Fe is similar to a polymer with multiple (-Fe-O-) n Repeating unit.
[0030] The products of methane oxidative carbonylation include C1 product (mainly methanol and formic acid, formic acid is mainly produced by oxidation of methanol) and C2 product (acetic acid), and the generation of C1 and C2 products is a competitive reaction. The present invention introduces Cu species on the basis of Fe / ZSM-5 catalyst. The addition of Cu species inhibits the coupling of hydroxyl radicals and methyl radicals, thereby improving the selectivity of acetic acid.
[0031] The present invention provides a method for preparing the FeCu / ZSM-5 catalyst described in the above scheme, comprising the following steps: dissolving an iron salt and a copper salt in water to obtain a metal salt solution;
[0032] The ammonium ZSM-5 molecular sieve is mixed with the metal salt solution for vacuum impregnation, and the obtained impregnation liquid is rotary evaporated and dried to obtain a FeCu / ZSM-5 catalyst precursor; the masses of the Fe element and the Cu element in the metal salt solution are respectively equal to the masses of the Fe element and the Cu element in the target FeCu / ZSM-5 catalyst;
[0033] The FeCu / ZSM-5 catalyst precursor is calcined under static air to obtain the FeCu / ZSM-5 catalyst.
[0034] In the present invention, unless otherwise specified, the raw materials and equipment used are commercially available products well known in the art.
[0035] The invention dissolves iron salt and copper salt into water to obtain a metal salt solution.
[0036] The present invention has no special requirements for the iron salt and copper salt. Any water-soluble iron salt and copper salt known in the art can be used, such as nitrates, hydrochlorides, and acetylacetonate. In an embodiment of the present invention, the iron salt is specifically ferric nitrate nonahydrate, and the copper salt is specifically copper nitrate trihydrate.
[0037] The present invention has no special requirements on the concentration of the metal salt solution, as long as the iron salt and the copper salt can be completely dissolved and the volume of the metal salt solution is larger than the volume of the solution used for equal volume impregnation.
[0038] In the present invention, the amount of the iron salt and the copper salt is calculated based on the content of the Fe element and the Cu element in the target FeCu / ZSM-5 catalyst, and the masses of the Fe element and the Cu element in the metal salt solution are respectively equal to the masses of the Fe element and the Cu element in the target FeCu / ZSM-5 catalyst.
[0039] After obtaining the metal salt solution, the present invention mixes the ammonium ZSM-5 molecular sieve with the metal salt solution for vacuum impregnation, and the obtained impregnation liquid is rotary evaporated and dried to obtain a FeCu / ZSM-5 catalyst precursor.
[0040] In the present invention, the ammonium-type ZSM-5 molecular sieve is preferably obtained by exchanging ammonium ions with Na-type ZSM-5 molecular sieves; the present invention has no special requirements for the process of exchanging ammonium ions, and the ammonium ion exchange process well known in the art can be used. The active site of the catalyst is a mononuclear Fe species, which is located at the Bronsted acid site, replacing the position of proton H. If Na-ZSM-5 molecular sieve is used as a carrier, it will compete with the location of mononuclear Fe, so that the number of active sites is reduced.
[0041] In the present invention, the vacuum impregnation preferably includes: firstly subjecting the ammonium ZSM-5 molecular sieve to a first vacuum treatment under closed conditions, then injecting a metal salt solution to continue a second vacuum treatment, and finally stirring at room temperature.
[0042] In the present invention, the time of the first vacuum treatment is preferably 20 to 40 minutes, more preferably 30 minutes; the vacuum degree is preferably 0.05 to 0.1 MPa; the time of the second vacuum treatment is preferably 5 to 20 minutes, more preferably 10 minutes, and the vacuum degree is preferably 0.05 to 0.1 MPa. In the present invention, the stirring time is preferably 20 to 28 hours, more preferably 24 hours; the stirring rate is preferably 700 to 900 rpm, more preferably 800 rpm. The present invention uses vacuum impregnation to evenly disperse the metal elements on the ammonium ZSM-5 molecular sieve.
[0043] In the present invention, the temperature of the rotary evaporation is preferably 65-75° C., more preferably 70° C.; the present invention has no special requirements on the time of the rotary evaporation, as long as it can remove most of the water solvent.
[0044] In the present invention, the drying temperature is preferably 70-90° C., more preferably 80° C.; the present invention has no special requirements for the drying time, as long as the drying time is complete.
[0045] After obtaining the FeCu / ZSM-5 catalyst precursor, the present invention calcines the FeCu / ZSM-5 catalyst precursor under static air to obtain the FeCu / ZSM-5 catalyst.
[0046] In the present invention, the calcination temperature is preferably 500° C., and the temperature is maintained at 500° C. for 3 hours. The present invention promotes the decomposition of metal salts into metal oxides by calcination, wherein Fe exists in the form of Fe species, i.e., mononuclear Fe, oligomeric Fe and nano Fe2O3 particles, and Cu exists in the form of Cu species, i.e., mononuclear Cu.
[0047] The present invention provides the use of the FeCu / ZSM-5 catalyst described in the above scheme or the FeCu / ZSM-5 catalyst prepared by the preparation method described in the above scheme in catalyzing methane carbonylation reaction to produce acetic acid.
[0048] The present invention has no special requirements for the implementation process and reaction conditions of the methane carbonylation reaction to produce acetic acid, and the implementation process and reaction conditions known in the art can be used. In an embodiment of the present invention, the conditions for the methane carbonylation reaction to produce acetic acid include: the reaction temperature is preferably 50°C, the reaction time is preferably 0.5h, and the hydrogen peroxide concentration is preferably 0.5mol·L -1 The methane pressure is preferably 2.5 MPa, the carbon monoxide pressure is preferably 2.5 MPa, and the amount of catalyst used is preferably 30 mg.
[0049] The FeCu / ZSM-5 catalyst provided by the present invention, its preparation method and its application in catalyzing methane carbonylation reaction to produce acetic acid are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0050] Removal of organic templates from ZSM-5 molecular sieves:
[0051] Weigh 20g of purchased ZSM-5 molecular sieve raw powder, divide it into four evaporating dishes, and place it in a muffle furnace for calcination. Figure 1 The calcination was carried out at a heating rate of 1 °C / min and an air flow rate of 100 mL·min -1 The temperature at 120°C is to remove the water molecules adsorbed on the surface of the molecular sieve. After the calcination is completed, the mixture is cooled to room temperature naturally and then the muffle furnace is opened to take out the mixture, thereby obtaining Na-ZSM-5 with the organic template removed.
[0052] Preparation of ammonium ZSM-5 molecular sieve:
[0053] Transfer about 20 g of the Na-ZSM-5 molecular sieve obtained in the previous step and remove the organic template into a beaker, add 250 mL of 1 mol·L-1 NH4NO3 solution, ion exchange at 80℃ for 12h, stirring rate is 500rpm. Then centrifuge to separate the solid and liquid phases, decant the supernatant and add deionized water for washing, repeat the above steps four times, after completing four ion exchange steps, transfer the lower molecular sieve precipitate obtained by centrifugation to an evaporating dish, place it in an oven for drying, the drying temperature is 80℃, and the drying time is 12h. After drying, grind to obtain NH4-ZSM-5 molecular sieve powder.
[0054] Example 1
[0055] Dissolving ferric nitrate nonahydrate and copper nitrate trihydrate in water to obtain a metal salt solution;
[0056] Transfer 1.0g of NH4-ZSM-5 molecular sieve powder to a 100mL pear-shaped bottle, put in a magnetic stirrer and seal it with a rubber stopper, then vacuum it for 0.5h. Measure a certain amount of 0.1mol / L metal salt solution and dilute it to 15mL with ultrapure water. Use a syringe to inject the diluted metal salt solution into the pear-shaped bottle after the vacuum treatment. Wash the vessel and syringe with 1mL ultrapure water 2 to 3 times each time and transfer them to the pear-shaped bottle, and then continue the vacuum treatment for 10min. After stirring for 24h at room temperature, the impregnation is completed, the stirring rate is 800rpm, and then the most of the solvent is removed by rotary evaporation at 70℃, and then placed in an oven for thorough drying at 80℃ and 12h. After grinding the obtained powder, transfer it to an evaporating dish and place it in a muffle furnace for calcination under static air at a calcination temperature of 500℃ and a calcination time of 3h. After the calcination is completed, wait for it to cool naturally to room temperature, open the muffle furnace and take it out to obtain (Fe 0.5 Cu 0.1 ) / ZSM-5, where Fe 0.5 The loading amount of metal element Fe on the catalyst is 0.5wt%, that is, [Fe mass / (molecular sieve mass+theoretical Fe2O3 mass+theoretical CuO mass)]×100%, Cu 0.1 It means that the loading amount of metal element Cu on the catalyst is 0.1wt%, that is, [mass of Cu / (mass of molecular sieve+theoretical mass of Fe2O3+theoretical mass of CuO)]×100%.
[0057] Example 2
[0058] The only difference from Example 1 is that the Cu loading is 0.15 wt % and the obtained catalyst is denoted as (Fe 0.5 Cu 0.15 ) / ZSM-5.
[0059] Example 3
[0060] The only difference from Example 1 is that the Cu loading is 0.2 wt % and the obtained catalyst is denoted as (Fe 0.5 Cu 0.2 ) / ZSM-5.
[0061] Example 4
[0062] The only difference from Example 1 is that the Cu loading is 0.25 wt % and the obtained catalyst is denoted as (Fe 0.5 Cu 0.25 ) / ZSM-5.
[0063] Comparative Example 1
[0064] The only difference from Example 1 is that the Cu loading is 0.5 wt % and the obtained catalyst is denoted as (Fe 0.5 Cu 0.5 ) / ZSM-5.
[0065] Comparative Example 2
[0066] The only difference from Example 1 is that the Cu loading is 0.05 wt % and the obtained catalyst is denoted as (Fe 0.5 Cu 0.05 ) / ZSM-5.
[0067] Comparative Example 3
[0068] The only difference from Comparative Example 1 is that no Cu is loaded, and the obtained catalyst is recorded as Fe 0.5 / ZSM-5.
[0069] Comparative Example 4
[0070] The only difference from Comparative Example 1 is that no Fe is loaded, and the obtained catalyst is recorded as Cu 0.5 / ZSM-5.
[0071] Comparative Example 5
[0072] The difference from Comparative Example 1 is that the order of introducing the active components is changed. Fe is first loaded by vacuum impregnation and calcined, and then Cu is loaded by vacuum impregnation and calcined. The obtained catalyst is recorded as Fe 0.5 -Cu 0.5 / ZSM-5.
[0073] Comparative Example 6
[0074] The difference from Comparative Example 1 is that the order of introducing the active components is changed. First, the Cu is loaded by vacuum impregnation and calcined, and then the Fe is loaded by vacuum impregnation and calcined. The obtained catalyst is recorded as Cu 0.5 -Fe 0.5 / ZSM-5.
[0075] Structure and performance characterization:
[0076] The catalysts prepared in Comparative Example 1 and Comparative Examples 3 to 6 were characterized by powder X-ray diffraction (PXRD). Figure 2 As shown. Figure 2 It can be seen that with the loading of Fe and Cu, the MFI structure of the ZSM-5 molecular sieve is well maintained, and no diffraction peaks of Fe2O3 and CuO are observed, indicating that Fe and Cu are well dispersed on the ZSM-5 molecular sieve framework, and the particle size of Fe species and Cu species is smaller than the PXRD detection limit (about 4nm).
[0077] Further Cu 0.5 The UV-visible spectroscopy analysis of the ZSM-5 catalyst showed that Figure 3 As shown in the figure (the horizontal axis is wavelength, in nm; the vertical axis is absorption intensity), it is confirmed that Cu species mainly exist in two forms: tetrahedral mononuclear Cu (210nm) and octahedral mononuclear Cu (278nm). The existence form of Cu species is related to the Cu loading amount. Figure 3 It is inferred that the (Fe 0.5 Cu 0.5 ) / ZSM-5 Cu mainly exists in the form of mononuclear Cu.
[0078] The existence form of Fe species is related to the Fe loading amount. When the Fe loading amount is high, the Fe species will have mononuclear Fe, oligomeric Fe and nano Fe2O3 particles. When the loading amount is low, there are generally only two forms of mononuclear Fe and oligomeric Fe. According to the inventor's previous paper "Oxidative carbonylation ofmethane to acetic acid on anFe-modifiedZSM-5zeolite", when the Fe loading amount is 0.25wt% to 1wt%, mononuclear Fe, oligomeric Fe and nano Fe2O3 particles exist at the same time. Therefore, when the Fe loading amount of the present invention is 0.5wt%, mononuclear Fe, oligomeric Fe and nano Fe2O3 particles will exist at the same time.
[0079] The catalytic performance of the catalysts of Comparative Example 1 and Comparative Examples 5-6 was compared. The conditions for the carbonylation of methane to produce acetic acid were: reaction temperature of 50°C, reaction time of 0.5h, hydrogen peroxide concentration of 0.5mol·L -1 , methane pressure is 2.5MPa, carbon monoxide pressure is 2.5MPa, and the amount of catalyst used is 30mg. The catalytic results are shown in Table 1.
[0080] Table 1 Reaction results of catalysts in Comparative Examples 1 and 5-6
[0081]
[0082] Note: In Table 1 (Fe 0.5 Cu 0.5 ) represents the (Fe 0.5 Cu 0.5 ) / ZSM-5,Fe 0.5 -Cu 0.5 Fe represents Comparative Example 5 0.5 -Cu 0.5 / ZSM-5,Cu 0.5 -Fe 0.5 Cu representing Comparative Example 6 0.5 -Fe 0.5 / ZSM-5.
[0083] As shown in Table 1, the order of introduction of Cu has a great influence on the performance of Fe and Cu loaded ZSM-5 catalysts. Compared with the catalyst loaded with Fe first, the acetic acid yield of the catalyst loaded with Cu first is greatly reduced. It is speculated that this is because Cu preferentially occupies the loadable sites on the ZSM-5 molecular sieve, thus greatly reducing the content of mononuclear Fe species and thus greatly reducing the activity of the catalyst. The catalyst prepared by loading Cu and Fe at the same time has the highest selectivity for acetic acid.
[0084] The catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 3 with different Cu loadings were used for methane carbonylation to produce acetic acid at a reaction temperature of 50° C., a reaction time of 0.5 h, and a hydrogen peroxide concentration of 0.5 mol·L -1 , methane pressure is 2.5MPa, carbon monoxide pressure is 2.5MPa, and the amount of catalyst used is 30mg. The reaction results are shown in Figure 4 and Table 2.
[0085] Table 2 Reaction results of catalysts in Examples 1 to 4 and Comparative Examples 1 to 3
[0086]
[0087] Depend on Figure 4 As shown in Table 2, when the Cu loading is 0.1-0.25wt%, the selectivity of acetic acid is greatly improved, reaching a maximum of 70.1%; when the Cu loading is above 0.25wt%, the peroxidation of methanol is greatly inhibited, and no formic acid is observed in the product, but because the formation of acetic acid is also greatly inhibited, the selectivity of acetic acid decreases. Similarly, from the changes in carbon dioxide, it can be seen that the introduction of Cu greatly inhibits the side reaction of hydrogen peroxide oxidizing carbon monoxide. With the increase of Cu loading, the yield of carbon dioxide has been decreasing. Comprehensively considered, when the Cu loading is between 0.1 and 0.25wt%, the catalytic performance is well improved.
[0088] In order to confirm the role of Cu in the carbonylation reaction of methane, the present invention uses a free radical scavenger DMPO to capture free radicals that may exist in the reaction process and characterizes them using electron paramagnetic resonance (EPR) spectroscopy. Figure 5 As shown, there is a typical quartet signal (a N =a H =14.9G) and g=2.0074, indicating that DMPO / ·OH adducts can be detected during the reaction. At the same time, the present invention keeps the same amount of DMPO added to qualitatively compare the differences in the generation of hydroxyl radicals by different catalysts. The results show that with the increase of Cu loading, the concentration of hydroxyl radicals increases by an order of magnitude, which is much higher than that of Fe without loading. 0.5 / ZSM-5 catalyst. It can be seen that the Cu species inhibits the conversion of hydroxyl radicals and methyl radicals, resulting in a higher concentration of hydroxyl radicals in the liquid phase.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A FeCu / ZSM-5 catalyst, It is characterized in that It comprises a ZSM-5 molecular sieve and an active component loaded on the ZSM-5 molecular sieve; The active components include Fe species and Cu species; the Fe species include mononuclear Fe, oligomeric Fe and nano Fe 2 O 3 particles; the Cu species comprises mononuclear Cu; The content of Fe element in the FeCu / ZSM-5 catalyst is 0.4-0.6 wt %, and the content of Cu element is 0.1-0.25 wt %.
2. The preparation method of the FeCu / ZSM-5 catalyst according to claim 1, The following steps are involved: Dissolving iron salt and copper salt in water to obtain a metal salt solution; The ammonium ZSM-5 molecular sieve is mixed with the metal salt solution for vacuum impregnation, and the obtained impregnation liquid is rotary evaporated and dried to obtain a FeCu / ZSM-5 catalyst precursor; the masses of the Fe element and the Cu element in the metal salt solution are respectively equal to the masses of the Fe element and the Cu element in the target FeCu / ZSM-5 catalyst; The FeCu / ZSM-5 catalyst precursor is calcined under static air to obtain the FeCu / ZSM-5 catalyst.
3. The preparation method according to claim 2, It is characterized in that The calcination temperature is 500° C. and maintained at 500° C. for 3 hours.
4. The preparation method according to claim 2, It is characterized in that The vacuum impregnation comprises: firstly subjecting the ammonium ZSM-5 molecular sieve to a first vacuum treatment under a closed condition, then injecting a metal salt solution to continue a second vacuum treatment, and finally stirring at room temperature.
5. The preparation method according to claim 4, It is characterized in that The first vacuum treatment lasts for 20 to 40 minutes, and the vacuum degree is 0.05 to 0.1 MPa.
6. The preparation method according to claim 4, It is characterized in that The second vacuum treatment lasts for 5 to 20 minutes, and the vacuum degree is 0.05 to 0.1 MPa.
7. The preparation method according to claim 4, It is characterized in that The stirring time is 20 to 28 hours, and the stirring speed is 700 to 900 rpm.
8. The preparation method according to claim 2, It is characterized in that The temperature of the rotary evaporation is 65-75°C; the temperature of the drying is 70-90°C.
9. The preparation method according to claim 2, It is characterized in that The ammonium type ZSM-5 molecular sieve is obtained by exchanging the Na type ZSM-5 molecular sieve with ammonium ions.
10. Use of the FeCu / ZSM-5 catalyst according to claim 1 or the FeCu / ZSM-5 catalyst prepared by the preparation method according to any one of claims 2 to 9 in catalyzing the carbonylation reaction of methane to produce acetic acid.