Flotation method for comprehensively recovering silver, zinc and lead from zinc smelting slag
By using grinding and flotation processes in zinc smelting slag combined with protective gas and alkaline regulators, the comprehensive recycling problem of silver, zinc and lead in zinc smelting slag is solved, and efficient metal recycling and process are achieved Stability reduces production costs.
Patent Information
- Application Number
- CN202411179525.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The comprehensive recycling problem of silver, zinc and lead in zinc smelting slag, especially the low flotation recycling efficiency of lead, and the traditional ignition process has high energy consumption and serious pollution, making it difficult to apply in places without lead smelting facilities, and acid-leaching waste slag The content of lead and silver is low, making it difficult to directly recover.
A low-cost flotation process is adopted, through the two steps of grinding, silver-zinc flotation and lead flotation, silver-zinc and lead flotation, the slurry is adjusted using protective gas and alkaline adjusters to drive away dissolved oxygen. Perform vulcanization treatment to improve the flotation effect of lead, and precipitate other metal ions through a large dose of alkaline adjuster to ensure the vulcanization effect.
It realizes the comprehensive recycling of low-cost silver, zinc and lead under normal temperature conditions, improves the recovery rate, stabilizes the process, reduces the cost of agents, and solves the problem of low utilization rate of metal components in zinc smelting slag.
Smart Images

Figure CN119016184A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of nonferrous metal solid waste, and in particular to a flotation process for recovering valuable metals from zinc smelting slag. Background Art
[0002] Zinc is an important raw material for nonferrous metals. About 85% of the total zinc smelting in the world is obtained through the hydrometallurgical zinc smelting process, in which the zinc sulfide concentrate is roasted and then leached with hot acid and high acid to obtain acid leaching waste slag. Every ton of electrolytic zinc produced produces about 0.3 tons of acid leaching waste slag, which contains a certain amount of metal elements such as lead, zinc, copper, silver, and cadmium. At present, zinc smelting slag is mainly stored in piles, which has strong environmental hazards and high disposal costs, but the metal components in it also have extremely high comprehensive recovery value. The methods for recovering metal elements from zinc smelting slag mainly include hydrometallurgical leaching, pyrometallurgical process, flotation and smelting combined process, among which pyrometallurgical process is the most commonly used comprehensive utilization method. For example, patent CN107326190B uses reduction roasting to change the state of valuable metals in the smelting slag containing lead, zinc and silver, and obtains high-grade PbO, ZnO smoke and roasting slag enriched with Ag. The smoke enters the lead and zinc smelting system; the roasting slag is refined by flotation of silver to obtain silver concentrate and tailings, and finally realizes the resource utilization of valuable metals. However, the use of pyrometallurgical furnace technology requires enterprises to have supporting facilities for lead smelting. In places where there is no lead smelting, this method is difficult to apply. In addition, traditional pyrometallurgical processes (such as rotary kilns, fuming furnace volatilization treatment, etc.) have high energy consumption and pollution. With the improvement of environmental protection requirements, the application of such methods is also subject to certain restrictions.
[0003] Since the content of lead and silver in acid leaching waste residue is relatively low, it is also difficult to directly recover lead and silver by traditional wet leaching. The flotation process has the advantages of simple process flow, low investment and low production cost, and is an effective way to achieve comprehensive recovery and disposal of acid leaching waste residue. For example, patent CN109261347B uses a new collector for mixed flotation after ultrasonic activation of smelting waste residue to obtain mixed flotation concentrate. For this reason, smelting enterprises often use flotation to recover precious metals in acid leaching waste residue, especially the recovery of silver in zinc leaching residue. However, since most of the lead in smelting slag exists in the form of difficult-to-float silicates, sulfates and oxides, the acid leaching waste residue contains a large amount of impurity ions, among which the flotation recovery of lead has always been a technical problem in the industry. Therefore, how to achieve the comprehensive recovery of silver, zinc and lead in zinc smelting slag at room temperature through a low-cost flotation process has important practical guiding significance. Summary of the invention
[0004] The purpose of the present invention is to provide a flotation process for recovering silver, zinc and lead from zinc smelting slag with low cost and simple process, and to enhance the lead flotation effect by introducing protective gas, adjusting agent and other slurry adjustment in the lead flotation link.
[0005] The purpose of the present invention is achieved by the following methods:
[0006] A flotation method for comprehensively recovering silver, zinc and lead from zinc smelting slag comprises the following steps:
[0007] (1) Grinding: Grinding zinc smelting slag slurry;
[0008] (2) Silver and zinc flotation: Adding adjusting agent I, collecting agent I and frother to the ore pulp, and then flotation to obtain silver and zinc concentrates;
[0009] (3) Lead flotation: For the tailings after the silver and zinc flotation in step (2), a protective gas is pre-filled to stir and slurry, and then a regulator II is added under the protection of a protective atmosphere, and then a sulfiding agent is added to the slurry for sulfidation. After sulfidation, a collector II and a frother are added, and then flotation is performed to obtain a lead concentrate.
[0010] Further,
[0011] The zinc smelting slag slurry described in step (1) is prepared by adding water to zinc smelting slag, and the mass concentration is 20% to 50%.
[0012] Furthermore,
[0013] The zinc smelting slag described in step (1) comes from a filter press sample of high-acid leaching slag from a zinc smelter, and water-soluble zinc in the zinc smelting slag is recovered by pulp washing before filter press.
[0014] In step (1), the grinding fineness is -0.074 mm and the content is more than 50%.
[0015] Further,
[0016] In step (2), the adjusting agent I is at least one of water glass, sodium hexametaphosphate, copper sulfate and sodium sulfide; the amount of water glass, at least one of sodium hexametaphosphate and copper sulfate is at least 300g / t of zinc smelting slag dry slag, preferably in the range of 300-600g / t of zinc smelting slag dry slag; the amount of sodium sulfide is at least 500g / t of zinc smelting slag dry slag, preferably in the range of 800-1600g / t of zinc smelting slag dry slag.
[0017] The collector I is at least one of butyl ammonium black powder, No. 25 black powder, No. 31 black powder, and butyl ammonium yellow powder, and the dosage is at least 300g / t of dry zinc smelting slag; the preferred dosage range is 500-800g / t of dry zinc smelting slag.
[0018] Further,
[0019] In step (3), protective gas is pre-filled to adjust the slurry to drive away the dissolved oxygen in the slurry (the dissolved oxygen concentration in the slurry is reduced to within 2.0 mg / L, preferably controlled at 0.8-1.5 mg / L); and the filling of protective gas is stopped after the addition of the adjusting agent II and before the addition of the sulfiding agent.
[0020] Furthermore,
[0021] In step (3), the adjusting agent II is at least one of sodium citrate and disodium ethylenediaminetetraacetate and sodium carbonate; the amount of at least one of sodium citrate and disodium ethylenediaminetetraacetate is at least 300 g / t of dry zinc smelting slag; the amount of sodium carbonate is at least 1000 g / t of dry zinc smelting slag. The preferred amount range of sodium carbonate is 5000-10000 kg / t of dry zinc smelting slag; the preferred amount of at least one of sodium citrate and sodium ethylenediaminetetraacetate is 500-1300 g / t of dry zinc smelting slag.
[0022] The present invention finds that the reason why the flotation of lead in zinc smelting slag by sulfidation is not ideal is the presence of oxygen in the system. Therefore, a protective gas is used for the first time to adjust the slurry system before sulfidation to drive away the dissolved oxygen in the slurry, which will greatly improve the effect of sulfidation flotation of lead.
[0023] In addition, the present invention adopts a large dose of alkaline adjusting agent for the first time, especially the addition of sodium carbonate, which can not only effectively precipitate other metal ions, but also continuously produce a large amount of carbon dioxide. After the introduction of protective gas is stopped, it continues to provide support for the anaerobic environment, thereby providing a guarantee for the subsequent vulcanization effect.
[0024] In step (3), the sulfiding agent is at least one of sodium sulfide and sodium hydrosulfide, and the dosage is at least 1000 g / t of high acid leaching slag from a zinc smelter, and the preferred dosage range of the sulfiding agent is 5000-20000 kg / t; the collector II includes at least one of amyl xanthate, octyl xanthate, and mercaptobenzothiazole, and the dosage is at least 300 g / t of dry zinc smelting slag, and the preferred dosage is 600-800 g / t of dry zinc smelting slag.
[0025] Further,
[0026] The foaming agent used in steps (2) and (3) is at least one of 2# oil, pine oil, MIBC and butyl ether alcohol, and the amount used is at least 10 g / t of dry zinc smelting slag; the preferred amount range is 10-20 g / t of dry zinc smelting slag.
[0027] By the above method, silver-zinc concentrate with a silver grade of 700-1000 g / t, a zinc grade of 6-8%, a silver recovery rate of 69-74%, and a zinc recovery rate of 35-40% can be obtained, as well as a lead concentrate with a lead grade of 19-23% and a lead recovery rate of 65-70%.
[0028] The zinc smelting slag dry slag of the present invention is obtained by drying the filter press sample of the high acid leaching slag of the zinc smelting plant to a constant weight. In the actual production process, the filter press sample with moisture after the smelting slag is directly used, not the dry slag. The dry slag is used to facilitate the description of the dosage of the reagent.
[0029] The advantages of the present invention are:
[0030] 1. In view of the characteristics of zinc smelting slag, which is highly acidic, fine in particle size, rich in valuable metals but difficult to recover, a flotation process flow of silver and zinc flotation under acidic conditions and lead flotation under weak alkaline environment was proposed through the regulation of pulp potential and pH. The operation is continuous and highly operable.
[0031] 2. In the lead flotation process, the dissolved oxygen in the ore pulp is driven away by protective gas, the lead mineral is sulfided by a sulfiding agent, and finally the lead is collected by a collector, which reduces the cost of reagents.
[0032] 3. Use large doses of alkaline adjusters to effectively precipitate metal ions such as iron, zinc, and calcium, continuously produce large amounts of carbon dioxide, and work in conjunction with protective gases to provide protection for subsequent vulcanization effects.
[0033] 4. This method has the characteristics of stable process flow and low cost, which solves the problem of low comprehensive recovery and utilization rate of silver, zinc and lead in zinc smelting slag, and realizes partial consumption of zinc smelting slag.
[0034] The following descriptions and embodiments in combination with the accompanying drawings are intended to further illustrate the present invention, but will not limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a test flow chart of Example 1 of the present invention; DETAILED DESCRIPTION
[0036] The raw ore used in the following examples and comparative examples is a sample of high-acid leaching slag filter press from a zinc smelter in Yunnan. Before filter press, the plant has recovered water-soluble zinc in the smelting slag by pulp washing. In the embodiment, the silver grade of the smelting slag is about 256g / t, the zinc grade is about 4.38%, and the lead grade is about 8.50%. The sodium sulfide used is industrial sodium sulfide with a purity of about 60%. The sodium carbonate used is industrial sodium carbonate with a purity of ≥98.8%. The amyl xanthate used is industrial grade with a purity of ≥99%. The water glass used is industrial grade with a purity of ≥99%. The pine oil used is industrial grade with a purity of ≥99%. The nitrogen used is pure ≥99%.
[0037] Example 1
[0038] The experimental flow chart of this embodiment is shown in Figure 1 , the detailed steps are as follows:
[0039] (1) After the raw ore is slurried at a concentration of 30%, it is ball milled for 2 minutes, and the grinding fineness is -0.074mm and the content is more than 50%.
[0040] 300 g / t of copper sulfate, 300 g / t of sodium hexametaphosphate and 1000 g / t of sodium sulfide were added, and the reaction lasted for 3 min. Then 800 g / t of butyl ammonium black powder and 15 g / t of pine oil were added, and the reaction lasted for 3 min. Then, silver and zinc were roughly separated for 6 min to obtain silver-zinc concentrate.
[0041] (2) Nitrogen is heated to 0.2m 3 / h flow rate was charged into the slurry for pretreatment for 4 minutes, and the dissolved oxygen concentration of the slurry was 2.0mg / L. Then 1000g / t of sodium citrate and 8000g / t of sodium carbonate were added, and the reaction lasted for 3 minutes. The pH of the slurry was adjusted to 6.4, and the potential was 320mV. At this time, the nitrogen filling was stopped, and 10Kg / t of sodium sulfide was added to the slurry, and the reaction lasted for 3 minutes. The pH of the slurry was adjusted to 7.5, and the potential was 40mV. Finally, 800g / t of amyl xanthate and 15g / t of pine oil were added, and the reaction lasted for 3 minutes.
[0042] (3) After the above steps are completed, lead roughing is carried out for 8 minutes to obtain lead concentrate.
[0043] The test results of Example 1 are shown in Table 1.
[0044] Table 1 Experimental results of Example 1
[0045]
[0046] Comparative Example 1
[0047] The difference between Comparative Example 1 and Example 1 is that no nitrogen is used in Comparative Example 1, and the other test conditions are completely the same.
[0048] The test results of Comparative Example 1 are shown in Table 2.
[0049] Table 2 Comparative Example 1 Test Results
[0050]
[0051] It can be seen from the results in Table 2 that when nitrogen is not used, the silver and lead grades decrease compared with Example 1, especially the lead recovery rate decreases significantly.
[0052] Comparative Example 2
[0053] The difference between Comparative Example 2 and Example 1 is that, in Comparative Example 2, the nitrogen is terminated before adding water glass, sodium citrate and sodium carbonate, and the other experimental conditions are completely the same.
[0054] The test results of Comparative Example 1 are shown in Table 3.
[0055] Table 3 Comparative Example 2 Test Results
[0056]
[0057] It can be seen from the results in Table 3 that when the nitrogen is stopped prematurely, the lead grade and lead recovery rate of the lead concentrate are both significantly reduced compared with Example 1.
[0058] Comparative Example 3
[0059] The difference between Comparative Example 3 and Example 1 is that the amount of sodium carbonate used in Comparative Example 3 is 6000 g / t, the pH is 6.0, and the other test conditions are completely the same.
[0060] The test results of Comparative Example 3 are shown in Table 4.
[0061] Table 4 Comparative Example 3 Test Results
[0062]
[0063] It can be seen from the results in Table 4 that when the amount of sodium carbonate is reduced, the lead grade and lead recovery rate of the lead concentrate are significantly reduced compared with Example 1.
[0064] Example 2
[0065] The detailed steps of this embodiment are as follows:
[0066] (1) After the raw ore is slurried at a concentration of 30%, it is ball milled for 2 minutes, and the grinding fineness is -0.074mm and the content is more than 50%.
[0067] 300 g / t of copper sulfate, 300 g / t of sodium hexametaphosphate and 1000 g / t of sodium sulfide were added, and the reaction lasted for 3 min. Then 800 g / t of butyl ammonium black powder and 15 g / t of pine oil were added, and the reaction lasted for 3 min. Then, silver and zinc were roughly separated for 6 min to obtain silver-zinc concentrate.
[0068] (2) Nitrogen is heated to 0.2m 3 / h flow rate was charged into the slurry for pretreatment for 4 minutes, and the dissolved oxygen concentration of the slurry was 2.0mg / L. Then 1000g / t of sodium citrate and 9000g / t of sodium carbonate were added, and the reaction lasted for 3 minutes. The pH of the slurry was adjusted to 6.5, and the potential was 310mV. At this time, the nitrogen filling was stopped, and 11Kg / t of sodium sulfide was added to the slurry, and the reaction lasted for 4 minutes. The pH of the slurry was adjusted to 7.7, and the potential was 33mV. Finally, 800g / t of amyl xanthate and 15g / t of pine oil were added, and the reaction lasted for 3 minutes.
[0069] (3) After the above steps are completed, lead roughing is carried out for 8 minutes to obtain lead concentrate.
[0070] The test results are shown in Table 5.
[0071] Table 5 Experimental results of Example 2
[0072]
[0073] Comparative Example 4
[0074] The difference between Comparative Example 2 and Example 2 is that, in Comparative Example 2, the pH and the pulp potential are modulated to the same level as in Example 2 by adjusting the dosage of the reagent without using nitrogen.
[0075] (1) After the raw ore is pulped at a concentration of 30%, it is ground with iron balls for 2 minutes, and the grinding fineness is -0.074mm and the content is more than 50%.
[0076] 300 g / t of copper sulfate, 300 g / t of sodium hexametaphosphate and 1000 g / t of sodium sulfide were added, and the reaction lasted for 3 min. Then 800 g / t of butyl ammonium black powder and 15 g / t of pine oil were added, and the reaction lasted for 3 min. Then, silver and zinc were roughly separated for 6 min to obtain silver-zinc concentrate.
[0077] (2) First, add 1000g / t of sodium citrate and 9500g / t of sodium carbonate, react for 3 minutes, adjust the pH of the pulp to 6.5, and the potential to 310mV. Then add 16Kg / t of sodium sulfide to the pulp, react for 4 minutes, adjust the pH of the pulp to 7.7, and the potential to 33mV. Finally, add 800g / t of amyl xanthate and 20g / t of pine oil, and react for 3 minutes.
[0078] (3) After the above steps are completed, lead roughing is carried out for 8 minutes to obtain lead concentrate.
[0079] The test results of Comparative Example 4 are shown in Table 6.
[0080] Table 6 Comparative Example 4 Test Results
[0081]
[0082] From the results in Table 6, it can be seen that when nitrogen is not used, Comparative Example 4 uses 500 g / t more sodium carbonate and 5000 g / t sodium sulfide, and adjusts the pH and pulp potential to the same level as Example 2. Compared with Example 2, the lead grade and lead recovery rate of the lead concentrate in Comparative Example 2 are significantly reduced.
[0083] Comparative Example 5
[0084] The difference between Comparative Example 5 and Example 2 is that the dosage of sodium citrate in Comparative Example 5 is 300 g / t, and the other test conditions are completely the same.
[0085] The test results of Comparative Example 5 are shown in Table 7.
[0086] Table 7 Comparative Example 5 Test Results
[0087]
[0088] It can be seen from the results in Table 7 that when the amount of sodium citrate is reduced, the lead grade and lead recovery rate of the lead concentrate are slightly reduced compared with Example 2.
Claims
1. A flotation method for comprehensively recovering silver, zinc and lead from zinc smelting slag, characterized in that: The following steps are involved: (1) Grinding: Grinding zinc smelting slag slurry; (2) Silver and zinc flotation: Adding adjusting agent I, collecting agent I and frother to the ore pulp, and then flotation to obtain silver and zinc concentrates; (3) Lead flotation: For the tailings after the silver and zinc flotation in step (2), a protective gas is pre-filled to stir and slurry, and then a regulator II is added under the protection of a protective atmosphere, and then a sulfiding agent is added to the slurry for sulfidation. After sulfidation, a collector II and a frother are added, and then flotation is performed to obtain a lead concentrate.
2. The method according to claim 1, characterized in that: The zinc smelting slag slurry described in step (1) is prepared by adding water to zinc smelting slag, and the mass concentration is 20% to 50%.
3. The method according to claim 1 or 2, characterized in that: The zinc smelting slag described in step (1) comes from a filter press sample of high-acid leaching slag from a zinc smelter, and water-soluble zinc in the zinc smelting slag is recovered by pulp washing before filter press.
4. The method according to claim 1, characterized in that: In step (1), the grinding fineness is -0.074 mm and the content is more than 50%.
5. The method according to claim 1, characterized in that: In step (2), the adjusting agent I is at least one of water glass, sodium hexametaphosphate, copper sulfate and sodium sulfide, and the amount of at least one of water glass, sodium hexametaphosphate and copper sulfate is at least 300g / t of dry zinc smelting slag; the amount of sodium sulfide is at least 500g / t of dry zinc smelting slag. The collector I is at least one of butyl ammonium black powder, No. 25 black powder, No. 31 black powder and butyl ammonium yellow powder, and the dosage is at least 300g / t of zinc smelting slag dry slag.
6. The method according to claim 1, characterized in that: In step (3), protective gas is pre-filled to adjust the slurry to drive away the dissolved oxygen in the slurry; and the filling of protective gas is stopped after the adjustment agent II is added for reaction and before the sulfiding agent is added.
7. The method according to claim 1 or 6, characterized in that: In step (3), the adjusting agent II is at least one of sodium citrate and disodium ethylenediaminetetraacetate and sodium carbonate; the amount of at least one of sodium citrate and disodium ethylenediaminetetraacetate is at least 300 g / t of dry zinc smelting slag; the amount of sodium carbonate is at least 1000 g / t of dry zinc smelting slag.
8. The method according to claim 1, 6 or 7, characterized in that: In step (3), the sulfiding agent is at least one of sodium sulfide and sodium hydrosulfide, and the amount used is at least 1000 g / t of dry zinc smelting slag; the collector II includes at least one of amyl xanthate, octyl xanthate, and mercaptobenzothiazole, and the amount used is at least 300 g / t of dry zinc smelting slag.
9. The method according to claim 1, characterized in that: The foaming agent used in steps (2) and (3) is at least one of 2# oil, pine oil, MIBC and butyl ether alcohol, and the amount used is at least 10 g / t of dry zinc smelting slag.
Citation Information
Patent Citations
A method for resource utilization of lead-zinc-silver smelting slag
CN107326190B
A method for resource utilization of lead-zinc smelting waste residue
CN109261347B
Technology for recovering lead, zinc, carbon, silver and iron from zinc smelting leaching residues
CN108531740A
Method of controlling oxidation-flotation recovery of galena
CN110064509A
Method for preparing high-purity pyrite through flotation mass transfer kinetics regulation and control
CN113976331A
Cited By
A method for synergistic activation and flotation of lead and silver metals in a high-chlorine water environment