Spraying method for durable coating on inner wall of roasting furnace
Through surface treatment and strain monitoring technology, combined with tungsten carbide coating spraying, the problem of insufficient bonding force between the inner wall coating of the calcinerator and the substrate is solved, and the durability of the coating and the overall durability of the calcinerator are improved.
Patent Information
- Application Number
- CN202310601724.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively improve the bonding force between the coating and the substrate in the high temperature and high pressure environment of the inner wall of the roasting furnace, resulting in insufficient durability of the coating and ineffective corrosion damage.
Remove the residual weld height by surface treatment, use high-temperature strain gauge to monitor deformation of key parts, conduct water pressure circulation and thermal stability cycle experiments, determine the strain stability value and minimum strain rate, and combine with corrosion-resistant coatings such as tungsten carbide to ensure the coating Close bond with the substrate.
It significantly improves the bonding force between the coating and the substrate, extends the service life of the coating, reduces the corrosion damage of the inner wall of the calcinerator, and improves the overall durability of the calcinerator.
Smart Images

Figure CN119016313A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion coatings, and in particular relates to a method for spraying a durable coating on the inner wall of a roasting furnace. Background Art
[0002] The calcining furnace is a commonly used equipment in the chemical industry. It is used for high-temperature synthesis, calcination, sintering, ashing, incineration, melting and heat treatment of various solid materials. It can significantly reduce the sintering temperature and greatly reduce energy consumption.
[0003] The roasting furnace is also one of the key equipment in the production process of molecular sieve catalysts. In the industrial production of catalysts, the roasting process is one of the important links. The working environment of the roasting furnace is usually around 800°C, which poses challenges to the long-term operation of the equipment, especially the cylinder. During the roasting process, a large amount of corrosive gases such as ammonia will be introduced into the roasting furnace, which will cause corrosive damage to the inner wall of the roasting furnace cylinder, and these corrosive damage and other problems will directly lead to the service life of the roasting furnace. Yu Wenxi and others analyzed the causes of furnace cracking through metallographic analysis and found that the main causes of furnace failure were thermal fatigue caused by thermal cycles due to material degradation caused by oxidation corrosion and creep. Zhang Yifan and others found that the fracture sites are mostly concentrated in the supporting parts, and factors such as bending stress and temperature difference stress are the main factors leading to furnace fracture. To prevent corrosion and other damage, it is necessary to spray the inner wall coating of the furnace.
[0004] How to ensure the durability of the coating in weak parts such as the roasting furnace barrel and welds under start-up and shutdown and high temperature and high pressure conditions is very important. In the current technology, the method of improving the bonding strength between the coating and the substrate is mainly to use a base coating of the same material as the substrate, or to add a transition layer to reduce the difference in thermal deformation between the substrate deformation and the coating. Patent CN110983229A discloses a coating for thermal protection of nickel-based high-temperature alloys and a preparation method thereof. Although the coating used for thermal protection of nickel-based high-temperature alloys can reach a temperature of 1400°C and has good thermal shock resistance, it does not consider the problem of deformation mismatch between the coating and the substrate, and the bonding strength between the coating and the substrate is not good enough. Patent CN114318207A discloses a method for preparing an atmospheric plasma sprayed metal alloy thermal barrier coating and its corresponding copper alloy substrate. The method combines a transition layer with a heat insulation layer so that the coating can fit closely to the surface of the substrate, and at the same time uses the transition layer to reduce the difference in thermal expansion between the substrate and the coating, but the substrate pretreatment is insufficient and the cost is relatively high.
[0005] There are relatively few methods for anti-corrosion coating of the inner wall of the roasting furnace. Therefore, it is necessary to provide a low-cost, simple and reliable technical method to solve the durability problem of the coating on the inner wall of the roasting furnace under harsh working conditions such as start-up and shutdown, high temperature and high pressure, especially the coating durability of the cylinder weld. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for spraying a durable coating on the inner wall of a roasting furnace, which can reduce the deformation mismatch problem between the coating and the substrate, improve the bonding force between the coating and the substrate, and extend the service life of the coating. The technical solution adopted is:
[0007] A method for spraying a durable coating on the inner wall of a roasting furnace, the specific steps comprising:
[0008] (1) Treat the inner wall of the roasting furnace to remove excess height and ensure surface roughness;
[0009] (2) Determine the key points of stress and strain in the roasting furnace, paste high-temperature strain gauges at the key points, and arrange strain monitoring at the key points;
[0010] (3) Set up a water pressure cycle experiment to determine the strain stability value;
[0011] (4) Thermal stability cycle test under pressure to determine the minimum strain rate;
[0012] (5) Corrosion-resistant coating spraying.
[0013] Preferably, in step (1), the specific method of surface treatment is to use an angle grinder in combination with a 220-mesh louvered blade to grind the excess height of the weld on the inner wall of the roasting furnace.
[0014] As a further preference, during grinding, the tangent direction of the louver blades is ground perpendicularly to the direction of the weld until the weld and the base material are in the same plane.
[0015] Preferably, in step (2), the critical stress and strain points of the roasting furnace are determined according to a method of thermo-solid coupling analysis of the roasting furnace.
[0016] As a further optimization, the thermo-solid coupling analysis method of the roasting furnace is to perform finite element modeling and simulation on the roasting furnace cylinder structure through ABAQUS simulation calculation software, consider the influence of thermal stress, pressure and gravity on the force of the cylinder structure, and determine the key points of stress and strain of the roasting furnace.
[0017] As a further preference, at least one high temperature strain gauge is attached to each of the key stress and strain points of the roasting furnace, and each strain gauge transmits an electrical signal to a collector through a cable. The collector calculates the deformation of the key points of the roasting furnace through the change in the resistance of the strain gauge.
[0018] Preferably, in step (3), the specific method of the water pressure test is to seal each outlet of the roasting furnace cylinder with a flange, inject water into the feed inlet, and inject water pressure to reach the maximum design pressure that the roasting furnace can withstand at a constant load rate;
[0019] After holding the load for 1 hour, slowly release the pressure to 0 MPa, and record the strain trend and maximum value of the high-temperature strain gauge through the data acquisition instrument;
[0020] Water pressure was injected again to reach the maximum design pressure that the roasting furnace could withstand at a constant load rate. After maintaining the load for 1 hour, the pressure was slowly released to 0 MPa. The strain operation trend and maximum value of the high-temperature strain gauge were recorded by the data acquisition instrument.
[0021] The maximum design pressure that the roasting furnace can withstand is 0.6MPa. The water pressure takes about 0.5h to reach 0.6MPa at a constant load rate. When the pressure is slowly released, it also takes about 0.5h to complete.
[0022] As a further preference, the water pressure cycle test is stopped when the strain operating trend of the high temperature strain gauge and the comparison of the maximum value before and after do not exceed 10%.
[0023] Preferably, in step (4), during the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, air is introduced for thermal circulation, and the creep test stress-strain curves of the roasting furnace body and the welded joint at a high temperature of 600°C are determined by high-temperature strain gauges.
[0024] As a further preference, the stress-strain curve is divided into three stages, the strain rate in the first stage gradually decreases, the strain rate in the second stage is constant, and the strain rate in the third stage increases.
[0025] As a further preference, when the creep strain enters the second stage, the high-temperature pressurized pre-operation time of the roasting furnace barrel is determined.
[0026] As a further preference, during the high-temperature pressurized pre-operation of the roasting furnace, the furnace is started and stopped multiple times to record the thermal strains of key points of the roasting furnace. When the thermal strains generated by each start and stop and the creep strains generated by the high-temperature pressurization do not exceed 10%, the operation is stopped.
[0027] Preferably, in step (5), the spraying includes pre-spraying and final spraying, and the sprayed coating is generally a corrosion coating such as tungsten carbide.
[0028] As a further preferred embodiment, the pre-spraying is performed by using a long-pole spray gun on the inner wall of the roasting furnace when the roasting furnace is pre-operated and slowly cooled from the working temperature of 600°C to 300°C;
[0029] The final spraying is performed on the inner wall of the roasting furnace by using a long-pole spray gun after the roasting furnace is completely cooled.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The method provided by the present invention requires grinding the weld and removing the excess height, so that the coating can be evenly sprayed on the inner wall of the roasting furnace cylinder, and the texture direction is perpendicular to the weld direction, avoiding becoming a subsequent crack source;
[0032] In the method provided by the present invention, the price of the high-temperature strain gauge used is relatively expensive. According to the finite element analysis results of the thermo-solid coupling calculation of the pressurized baking furnace, the high-temperature strain gauge can be specifically attached to the area with large deformation for monitoring, thereby reducing the cost;
[0033] In the method provided by the present invention, the material structure of the roasting furnace is strengthened by cyclic water pressure loading and unloading, and less deformation occurs during subsequent operation, the coating is better combined with the body, and the coating has higher durability;
[0034] In the method provided by the present invention, the stress generated by the local constraints of the roasting furnace is further released through multiple pressurized heat stabilization cycles, the strain is released, and the deformation of the key parts of the roasting furnace during service is reduced, so that the combination of the coating and the roasting furnace is more durable and firm;
[0035] The method provided by the present invention uses a corrosion-resistant coating such as tungsten carbide. Although the thermal expansion coefficients of the coating and the substrate are quite different, the coating may fall off during the thermal deformation process. The present invention starts spraying when the roasting furnace is not completely cooled, which can reduce the large deformation difference between the roasting furnace body and the coating after the roasting furnace is started, resulting in the coating falling off, thereby improving the bonding strength between the coating and the substrate and further improving the service life of the coating.
[0036] The method provided by the present invention is mainly used for large structural parts, which are in harsh service conditions, high temperature and high pressure conditions, and in corrosive environments, and need to adopt anti-corrosion coatings. Large welded structural parts have severe initial deformation under service conditions. Through pre-cycle overload and creep deformation, the structural performance of the structural parts under service conditions tends to be stable. The application scope includes but is not limited to baking furnaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a flow chart of the method of the present invention;
[0038] Figure 2 This is the creep test curve of the welded joint in Example 1. DETAILED DESCRIPTION
[0039] The drawings are for illustrative purposes only; in order to better illustrate the present embodiment, some parts of the drawings are omitted, enlarged or reduced, and do not represent the size of the actual product;
[0040] The orientations or positional relationships indicated by terms such as “upper”, “lower”, “top”, “bottom”, “side”, “outer”, “horizontal”, and “vertical” are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore should not be understood as limiting the present invention.
[0041] For those skilled in the art, some well-known structures and their descriptions in the drawings may be omitted, and therefore, they should not be understood as limitations of the present invention.
[0042] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0043] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0044] Example 1
[0045] like Figure 1 As shown, a method for spraying a durable coating on the inner wall of a roasting furnace needs to be processed and sprayed on the cylinder structure of a newly produced horizontal roasting furnace. The specific method includes:
[0046] The first step is to eliminate the internal weld of the cylinder, remove the excess height, and eliminate protrusions.
[0047] An angle grinder is used with a 220-mesh shutter blade to grind the weld excess height of the inner wall of the roasting furnace to ensure that the surface has a certain degree of roughness. The shutter blade tangent direction is perpendicular to the weld direction until the weld and the parent material are in the same plane. In this way, the coating can be sprayed evenly inside the roasting furnace cylinder, and the texture direction is perpendicular to the weld direction to avoid becoming a subsequent crack source.
[0048] Among them, for axial welds, the shutter blades swing back and forth along the circumferential direction for grinding; for circumferential welds, the shutter blades swing back and forth along the axial direction.
[0049] In the second step, a 1:1 solid model was established through ABAQUS simulation calculation software. The heat source was used for heating in the middle of the outside, forced convection and cavity radiation boundary conditions were imposed on the inner wall, and natural convection was carried out on the two ends of the outside with the outside world to carry out thermo-solid coupling analysis of the roasting furnace.
[0050] Roasting furnace shell size parameters:
[0051] Heating section 6000mm, insulation section 2×800mm, heating section thickness 300mm, non-insulation section 2×1000mm.
[0052] The inner diameter of the cylinder is 600mm, the outer diameter is 628mm, and the wall thickness is 28mm.
[0053] The heating section is 800℃, the cavity is radiant heat transfer, the radiation coefficient is 0.4, the heat loss caused by gas convection and materials is not considered, the insulation layer is glass fiber wool, the air convection coefficient is 0.005mW / mm2 / ℃, and the ambient temperature is 25℃.
[0054] Calculated load: thermal stress + internal pressure (0.6MPa) + gravity.
[0055] Since sequential coupling analysis is used, the heat transfer analysis unit type is DC3D8 and the stress analysis unit type is C3D8R.
[0056] The global layout is 50mm and the number of units in the thickness direction is 4.
[0057] Number of elements, 66156, number of nodes, 79681.
[0058] According to the results of literature research, the density, elastic modulus, Poisson's ratio, yield stress, thermal expansion coefficient, specific heat, and heat conduction parameters of N08810 material from room temperature to 1000°C were obtained.
[0059] For example, the material Incoloy 800HT has a density of 8g / cm3 and a thermal expansion coefficient of 15.0209×10-6 / ℃. The temperature variation curves of elastic modulus, yield stress, thermal expansion coefficient, specific heat, thermal conductivity, etc. can all be found.
[0060] The 1:1 solid model established by ABAQUS simulation software is subjected to mesh graphic analysis. A mesh transition is performed in the transition area from the heating section to the insulation section. The number of meshes in the thickness direction of the cylinder is not less than 6, and is set to 13 in this embodiment.
[0061] A fixed constraint is applied at one end of the cylinder to limit the rigid displacement, while preventing the constraint from being too large and affecting the calculation results of the concerned parts. The heat source, convection, thermal radiation, and changes in internal pressure are taken into account for the calculation.
[0062] Calculations show that the thermal stress in the transition area between the heat source and the exposed part is relatively large, reaching 60MPa.
[0063] At the same time, we carried out the baking furnace welding test plate 300*300*20mm 3 The simulation calculation of welding residual stress found that the residual stress of the weld and heat-affected zone was close to the yield stress value, and there was warping on both sides of the weld test plate, reaching 3°.
[0064] Therefore, the selection scheme for arranging high-temperature strain gauges at key points is as follows: select one weld on the outer wall of the roasting furnace, one heat-affected zone, one base material, and one temperature mutation site, and paste at least one strain gauge at each location.
[0065] Paste the high temperature strain gauge. The process includes:
[0066] First, use a thousand-blade grinder to grind the measured surface to remove surface burrs, rust layers and uneven pits. The grinding time is about 1 minute.
[0067] Since the grinding speed of the lapis lathe is too fast, it is easy to cause the surface to overheat. Therefore, after the lapis lathe is ground, it is polished with 220-grit sandpaper, cleaned with anhydrous alcohol, coated with high-temperature ceramic glue, and heated and cured with a hot air gun. The curing temperature is controlled at about 550°C (greater than the equipment operating temperature of 500°C), the curing time is 6 hours, and the high-temperature strain gauge is pasted;
[0068] The high temperature ceramic glue is applied again to the area around the high temperature strain gauge and cured using a hot air gun at a curing temperature of 300°C for 2 hours.
[0069] The strain gauge transmits the electrical signal to the collector through the cable. The collector calculates the deformation of the key points of the roasting furnace through the change of the strain gauge resistance, and the unit is μ strain.
[0070] The third step is to carry out water pressure circulation experiments to strengthen the roasting furnace cylinder structure.
[0071] The maximum design pressure that the roasting furnace can withstand is 0.6MPa, and the operating pressure is generally 0.3MPa.
[0072] Under laboratory conditions, each outlet of the roasting furnace cylinder was sealed with a flange, and water was injected into the main feed inlet. The water pressure was injected at a constant load rate (about 0.5h) to reach 0.6MPa. After maintaining the load for 1 hour, the pressure was slowly released to 0MPa (about 0.5h), and the strain operation trend and maximum value of the high-temperature strain gauge were recorded by the data acquisition instrument.
[0073] The strain value at the uniform base material is about 50 microstrain, the strain value at the heat affected zone is about 80 microstrain, and the strain value at the weld area is 40 microstrain; the water pressure is injected again, and after reaching 0.6MPa at a constant load rate (about 0.5h), the pressure is slowly released to 0MPa (about 0.5h) after maintaining the load for 1 hour, and the strain operation trend and maximum value of the high-temperature strain gauge are recorded by the data acquisition instrument. The strain value at the uniform base material is about 50 microstrain, the strain value at the weld is about 40 microstrain, and the strain value at the heat affected zone is about 100 microstrain; after 5 cycles, the strain value of the heat affected zone is maintained at about 110 microstrain and no longer increases, and the cyclic water pressure test is stopped.
[0074] The warping of the barrel caused by welding was almost flattened.
[0075] The fourth step is on-site high-temperature and pressure test operation. During the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, and air is introduced for heat circulation.
[0076] First, a high temperature creep test of a standard welded joint specimen was carried out. The creep curve consists of three stages, such as Figure 2 As shown, the percentage change of four creep strains with time is shown. Among them, the rate reduction stage (i.e. stage 1, time within 20 hours), the steady increase stage (i.e. stage 2, time within 20 to 580 hours, strain percentage within 2.1%), the accelerated increase stage (i.e. stage 3, time above 580 hours, strain percentage above 2.1%), the recorded rate reduction stage time is about 200 hours, which is preliminarily determined to be the high temperature pressure pre-operation time of the roasting furnace barrel.
[0077] The thermal strain and creep strain generated during the start-up of the key points of the roasting furnace were recorded by high-temperature strain gauges. The creep strain was small and the thermal strain was about 500 microstrain. During the high-temperature and pressurized pre-operation of the roasting furnace, it was started and stopped many times to record the thermal strain of the key points of the roasting furnace. When the start and stop reached 4 times, the difference between the microstrain before and after did not exceed 20 microstrain.
[0078] When the total running time reached 210h, the total strain curve of creep and thermal strain showed almost no increase, about 530 microstrain, then the operation was stopped and preparation for spraying began.
[0079] The fifth step is on-site spraying of tungsten carbide corrosion-resistant coating. When the roasting furnace is pre-operated and slowly cooled from the working temperature of 600℃ to 300℃, the inner wall of the roasting furnace is pre-sprayed by means of a long-pole spray gun. The long-pole spray gun is kept stationary, and the roasting furnace cylinder rotates at a constant speed through the movement of the bearing. The spraying thickness is about 300 microns. After one week of spraying, the long-pole spray gun moves forward a distance (about 3 cm).
[0080] After the roasting furnace is completely cooled, the final spraying of the inner wall of the roasting furnace is carried out, and the final coating thickness is inspected. The overall thickness of the coating is about 500 microns, and the error at each location does not exceed 20%.
[0081] After the roasting furnace ran for one cycle (three months), the inner wall was opened for inspection and it was found that the coating had not fallen off and the effect was good.
[0082] Comparative Example 1
[0083] Conventional tungsten carbide spraying, without pretreatment, directly sprays the tungsten carbide corrosion-resistant coating on site. When the roasting furnace is pre-operated and slowly cooled from the working temperature of 600℃ to 300℃, the inner wall of the roasting furnace is pre-sprayed by means of a long-pole spray gun. The long-pole spray gun is kept stationary, and the roasting furnace barrel rotates at a uniform speed through the movement of the bearing. The spraying thickness is about 300 microns. After one week of spraying, the long-pole spray gun moves forward a distance (about 3 cm).
[0084] After the roasting furnace is completely cooled, the final spraying of the inner wall of the roasting furnace is carried out, and the final coating thickness is inspected. The overall thickness of the coating is about 500 microns.
[0085] After two months of operation, the coating on the inner wall of the roasting furnace began to fall off, especially in the heat-affected zone of the weld, and corrosion began to appear.
[0086] Example 2
[0087] A method for spraying a durable coating on the inner wall of a roasting furnace, using manual arc welding to process a N08810 welding test plate, the size of the test plate is about 300*300*20mm 3 , V-notch, back root cleaning welding, the same as the baking furnace welding process, the weld is in the middle of the test plate. The specific steps include:
[0088] The first step is to use an angle grinder with a 220-mesh louvered blade to grind the weld excess height of the welding test plate to ensure that the surface has a certain degree of roughness.
[0089] The tangent direction of the louver blade is ground perpendicular to the weld direction until the weld is in the same plane as the base material.
[0090] Wire cutting, grinding and polishing are performed perpendicular to the weld direction to process standard tensile specimens.
[0091] The second step is to establish a 1:1 docking test plate model through ABAQUS simulation calculation software.
[0092] The weld adopts the "life and death unit" method, fixed heat source loading, double-sided single-pass welding. Natural convection and radiation conditions are applied to the boundary, with a radiation coefficient of 0.4, an air convection coefficient of 0.005mW / mm2 / ℃, and an ambient temperature of 25℃.
[0093] The sequential coupling analysis was adopted, the heat transfer analysis unit type was DC2D4, and the stress analysis unit type was GPE4R. The calculated residual stress at the plate butt joint was large, close to the yield strength of the material, 200MPa.
[0094] The third step is to carry out fatigue tests (0-60MPa) under tensile load on an MTS fatigue testing machine.
[0095] The experiment was stopped when the displacement displayed by the displacement sensor of the MTS fatigue testing machine no longer increased. The loading frequency was 1 Hz and the loading cycle was about 200 cycles.
[0096] The fourth step is to carry out a creep experiment with a preload of 260 MPa at 600 degrees Celsius on a creep testing machine. When the strain sensor of the creep testing machine shows that the strain has reached a stable value and no longer increases significantly in a short period of time (about 200 hours), the experiment is stopped.
[0097] Before spraying the tungsten carbide coating, sandblasting is performed to increase the roughness of the sample surface and increase the bonding strength between the coating and the substrate.
[0098] The fifth step is to carry out high temperature fatigue test on MTS fatigue testing machine after spraying tungsten carbide coating. The experimental process is to heat up to 600℃ at a rate of 300℃ / h, apply a load of 260MPa, maintain the load for 1 hour, air cool to room temperature, and repeat the cycle.
[0099] After 1000 hours of circulation, the coating remained intact without falling off.
[0100] Conventional tungsten carbide coating sprayed samples without pretreatment will fall off after running for 600 hours.
[0101] Therefore, by carrying out substrate pretreatment and reducing the deformation difference between the substrate and the coating, the durability of the coating can be significantly improved.
[0102] Example 3
[0103] A method for spraying a durable coating on the inner wall of a roasting furnace is used to pretreat and spray the coating to solve the problem of corrosion and shedding of the inner wall of a normal pressure horizontal rotary roasting furnace. The specific method includes:
[0104] The first step is to grind the "T"-shaped copy plate welding parts on the inner wall of the roasting furnace without structural mutations.
[0105] An angle grinder is used with a 220-mesh louver blade to grind the "T"-shaped copy plate welding part of the inner wall of the roasting furnace to ensure that the surface has a certain degree of roughness. First, the tangent direction of the louver blade is parallel to the weld direction, so that the weld and the parent material are in a smooth transition without structural discontinuities; then the tangent direction of the louver blade is perpendicular to the weld direction, and the texture direction is perpendicular to the weld direction to avoid becoming a subsequent crack source.
[0106] In the second step, a 1:1 model was established for welding simulation through ABAQUS simulation software. The structural dimensions of the "T" type copy plate are: 400mm long, 200mm wide, 10mm thick, and 28mm thick, which is simplified to a "T" type joint. The weld adopts the "life and death unit" method, fixed heat source loading, and double-sided single-pass welding. Natural convection and radiation conditions are applied to the boundary, with a radiation coefficient of 0.4, an air convection coefficient of 0.005mW / mm2 / ℃, and an ambient temperature of 25℃. Sequential coupling analysis is adopted, the heat transfer analysis unit type is DC2D4, and the stress analysis unit type is GPE4R.
[0107] The calculated residual stress of the “T”-type joint is relatively large, close to the yield strength of the material, 200 MPa.
[0108] Select the welding position where the middle of the "T"-shaped copy plate is connected to the cylinder, and paste the normal temperature strain gauge: at the weld, the heat affected zone of the copy plate and the heat affected zone of the cylinder, at least one strain gauge is pasted at each location.
[0109] Paste the high temperature strain gauge. The process includes:
[0110] First, use a thousand-blade grinder to grind the measured surface to remove surface burrs, rust layers and uneven pits. The grinding time is about 1 minute.
[0111] Since the grinding speed of the lapis lathe is too fast, it is easy to cause the surface to overheat. Therefore, after the lapis lathe is ground, it is polished with 200-grit sandpaper, cleaned with anhydrous alcohol, coated with high-temperature ceramic glue, and heated and cured with a hot air gun. The curing temperature is controlled at about 550°C (greater than the equipment operating temperature of 500°C), the curing time is 5 hours, and the high-temperature strain gauge is pasted;
[0112] The high temperature ceramic glue is applied again to the area around the high temperature strain gauge and cured using a hot air gun at a curing temperature of 300°C for 3 hours.
[0113] The strain gauge transmits the electrical signal to the collector through the cable. The collector calculates the deformation of the key points of the roasting furnace through the change of the strain gauge resistance, and the unit is μ strain.
[0114] The third step is to carry out mechanical circulation experiments to strengthen the welding parts of the internal plate structure of the roasting furnace.
[0115] The "T"-shaped joint copy plate is bent back and forth through a mechanical device, and the strain operating trend and maximum value of the strain gauge are recorded through a data acquisition instrument.
[0116] During a single bending, the strain value at the heat affected zone of the cylinder is about 10 microstrain, the strain value at the weld is about 100 microstrain, and the strain value at the heat affected zone of the copy plate is about 40 microstrain. The reciprocating bending amount is fixed, and after 5 cycles, the strain value at the heat affected zone of the cylinder is stabilized at 10 microstrain, the strain value at the weld is stabilized at 60 microstrain, and the strain value at the heat affected zone of the copy plate is stabilized at 18 microstrain.
[0117] The fourth step is on-site high-temperature trial operation. During the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, and air is introduced for heat circulation.
[0118] High-temperature creep experiments were carried out on standard welded joint specimens. The creep curve included three stages, namely, rate decrease stage, steady increase stage, and accelerated increase stage. The recorded time of the rate decrease stage was about 200 hours, which was preliminarily determined to be the high-temperature pressure pre-operation time of the roasting furnace shell.
[0119] The fifth step is on-site spraying of tungsten carbide-chromium carbide corrosion-resistant coating. When the roasting furnace is pre-operated and slowly cooled from the working temperature of 600℃ to 300℃, the "T" type copy plate welding part of the roasting furnace is pre-sprayed by means of a long-pole spray gun, and the spraying thickness is about 300 microns.
[0120] After the roasting furnace is completely cooled, the final spraying of the "T"-shaped copy board welding part of the inner wall of the roasting furnace is carried out, and the final coating thickness is inspected. The overall thickness of the coating is about 500 microns, and the error at each location does not exceed 18%.
[0121] After the roasting furnace had been running for one cycle (three months), it was opened for inspection and it was found that the coating on the "T"-shaped copy board inside the horizontal atmospheric pressure rotary roasting furnace had not fallen off, and the effect was good.
[0122] Example 4
[0123] Pretreatment and spraying of coating are carried out for the seriously corroded welds of the flange connection parts of the smoke outlet pipeline of the roasting furnace body. The specific methods include:
[0124] The first step is to process the internal welds of the newly processed export pipeline flange welding connection to remove excess height and eliminate protrusions.
[0125] The outlet pipeline has a diameter of 200mm, a wall thickness of 5mm, and is connected by flange welding. An angle grinder is used with a 220-mesh louver blade to grind the weld excess height of the inner wall of the flange welding part, while ensuring that the surface has a certain degree of roughness. The tangent direction of the louver blade is perpendicular to the weld direction until the weld is in the same plane as the parent material. In this way, the coating can be evenly sprayed inside the roasting furnace cylinder, and the texture direction is perpendicular to the weld direction to avoid becoming a subsequent crack source.
[0126] In the second step, a 1:1 axisymmetric model was established through ABAQUS simulation software for welding simulation. The welded joint is an axisymmetric structure with a thickness of 5mm, a diameter of 200mm, and a butt joint, which is simplified to a "V" notch form. The weld adopts the "life and death unit" method, fixed heat source loading, and double-sided single-pass welding. Natural convection and radiation conditions are imposed on the boundary, with a radiation coefficient of 0.4, an air convection coefficient of 0.005mW / mm2 / ℃, and an ambient temperature of 25℃. Sequential coupling analysis is adopted, the heat transfer analysis unit type is DC2D4, and the stress analysis unit type is GPE4R. The calculated residual stress at the welded joint of the pipe wall is large, close to the yield strength of the material of 200MPa.
[0127] Select the external parts of the outlet pipeline and flange connection welding, and paste the normal temperature strain gauges: at the weld, the heat affected zone of the copy plate and the heat affected zone of the cylinder, at least one strain gauge is pasted at each location.
[0128] When the strain gauge is pasted at room temperature, the process includes grinding with 220-grit sandpaper, cleaning the surface with anhydrous alcohol, applying strong glue, pressing and fixing, and baking with a hot air gun.
[0129] The strain gauge transmits the electrical signal to the collector through the cable. The collector calculates the deformation of the key points of the welding part of the copy plate through the change of the resistance of the strain gauge, and the unit is μ strain.
[0130] The third step is to carry out mechanical pulling and cyclic experiments to strengthen the welding parts between the export pipeline and the flange.
[0131] A large-tonnage universal testing machine is used to stretch and unload the flanged export pipeline. The stretching pressure is controlled at 60MPa, and the strain operating trend and maximum value of the high-temperature strain gauge are recorded by a data acquisition instrument.
[0132] The strain value at the uniform base material is about 300 microstrain, the strain value at the heat affected zone is about 220 microstrain, and the strain value at the weld area is 400 microstrain; after 5 cycles, the strain value at the uniform base material is about 310 microstrain, the strain value at the heat affected zone is about 240 microstrain, and the strain value at the weld area is 460 microstrain, and it no longer increases, so the cyclic experiment is stopped.
[0133] The fourth step is on-site high-temperature and pressure test operation. During the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, and air is introduced for heat circulation.
[0134] High-temperature creep experiments were carried out on standard welded joint specimens. The creep curve included three stages, namely, rate decrease stage, steady increase stage, and accelerated increase stage. The recorded time of the rate decrease stage was about 200 hours, which was preliminarily determined to be the high-temperature pressure pre-operation time of the roasting furnace shell.
[0135] The fifth step is spraying of tungsten carbide-chromium carbide corrosion-resistant coating. The export pipeline is heated as a whole. When it is heated to 300 degrees Celsius, it is taken out and pre-sprayed on the inner wall of the export pipeline by means of a long-pole spray gun. By moving the long-pole spray gun and rotating the export pipeline, the coating spray thickness is about 300 microns.
[0136] After the pipeline is completely cooled, the inner wall of the pipeline is finally sprayed and the final coating thickness is inspected. The overall thickness of the coating is about 500 microns, and the error at each location does not exceed 20%.
[0137] After the roasting furnace had been running for one cycle (three months), the flange of the roasting furnace outlet pipeline was opened to inspect the inner wall, and it was found that the coating had not fallen off, and the effect was good.
[0138] Example 5
[0139] A method for spraying a durable coating on the inner wall of a roasting furnace requires finishing and spraying the cylinder structure of a horizontal roasting furnace that has been used for a period of time. The specific method includes:
[0140] The first step is to eliminate the internal weld of the cylinder, remove the excess height, and eliminate protrusions.
[0141] An angle grinder is used with a 200-mesh shutter blade to grind the weld excess height of the inner wall of the roasting furnace to ensure that the surface has a certain degree of roughness. The shutter blade tangent direction is perpendicular to the weld direction until the weld and the parent material are in the same plane. In this way, the coating can be sprayed evenly inside the roasting furnace body, and the texture direction is perpendicular to the weld direction to avoid becoming a subsequent crack source.
[0142] Among them, for axial welds, the shutter blades swing back and forth along the circumferential direction for grinding; for circumferential welds, the shutter blades swing back and forth along the axial direction.
[0143] In the second step, a 1:1 solid model was established through ABAQUS simulation calculation software. The heat source was used for heating in the middle of the outside, forced convection and cavity radiation boundary conditions were imposed on the inner wall, and natural convection was carried out on the two ends of the outside with the outside world to carry out thermo-solid coupling analysis of the roasting furnace.
[0144] Roasting furnace shell size parameters:
[0145] Heating section 5000mm, insulation section 2×600mm, heating section thickness 300mm, non-insulation section 2×800mm.
[0146] The inner diameter of the cylinder is 500mm, the outer diameter is 628mm, and the wall thickness is 28mm.
[0147] The heating section is 800℃, the cavity is radiant heat transfer, the radiation coefficient is 0.4, the heat loss caused by gas convection and materials is not considered, the insulation layer is glass fiber wool, the air convection coefficient is 0.005mW / mm2 / ℃, and the ambient temperature is 25℃.
[0148] Calculated load: thermal stress + internal pressure (0.6MPa) + gravity.
[0149] Since sequential coupling analysis is used, the heat transfer analysis unit type is DC3D8 and the stress analysis unit type is C3D8R.
[0150] The global layout is 50mm and the number of units in the thickness direction is 4.
[0151] Number of elements, 66156, number of nodes, 79681.
[0152] According to the results of literature research, the density, elastic modulus, Poisson's ratio, yield stress, thermal expansion coefficient, specific heat, and heat conduction parameters of N08810 material from room temperature to 1000°C were obtained.
[0153] For example, the material Incoloy 800HT has a density of 8g / cm3 and a thermal expansion coefficient of 15.0209×10-6 / ℃. The temperature variation curves of elastic modulus, yield stress, thermal expansion coefficient, specific heat, thermal conductivity, etc. can all be found.
[0154] The 1:1 solid model established by ABAQUS simulation software is subjected to mesh graphic analysis. A mesh transition is performed in the transition area from the heating section to the insulation section. The number of meshes in the thickness direction of the cylinder is not less than 6, and is set to 10 in this embodiment.
[0155] A fixed constraint is applied at one end of the cylinder to limit the rigid displacement, while preventing the constraint from being too large and affecting the calculation results of the concerned parts. The heat source, convection, thermal radiation, and changes in internal pressure are taken into account for the calculation.
[0156] Calculations show that the thermal stress in the transition area between the heat source and the exposed part is relatively large, reaching 60MPa.
[0157] At the same time, we carried out the baking furnace welding test plate 300*300*20mm 3 The simulation calculation of welding residual stress found that the residual stress of the weld and heat-affected zone was close to the yield stress value, and there was warping on both sides of the weld test plate, reaching 3°.
[0158] Therefore, the selection scheme for arranging high-temperature strain gauges at key points is as follows: select one weld on the outer wall of the roasting furnace, one heat-affected zone, one base material, and one temperature mutation site, and paste at least one strain gauge at each location.
[0159] Paste the high temperature strain gauge. The process includes:
[0160] First, use a thousand-blade grinder to grind the measured surface to remove surface burrs, rust layers and uneven pits. The grinding time is about 2 minutes.
[0161] Since the grinding speed of the lapis lathe is too fast, it is easy to cause the surface to overheat. Therefore, after the lapis lathe is ground, it is polished with 220-grit sandpaper, cleaned with anhydrous alcohol, coated with high-temperature ceramic glue, and heated and cured with a hot air gun. The curing temperature is controlled at about 600°C (greater than the equipment operating temperature of 500°C), the curing time is 5 hours, and the high-temperature strain gauge is pasted;
[0162] The high temperature ceramic glue is applied again to the area around the high temperature strain gauge and cured using a hot air gun at a curing temperature of 300°C for 3 hours.
[0163] The strain gauge transmits the electrical signal to the collector through the cable. The collector calculates the deformation of the key points of the roasting furnace through the change of the strain gauge resistance, and the unit is μ strain.
[0164] The third step is to carry out water pressure circulation experiments to strengthen the roasting furnace cylinder structure.
[0165] The maximum design pressure that the roasting furnace can withstand is 0.6MPa, and the operating pressure is generally 0.3MPa.
[0166] Under laboratory conditions, each outlet of the roasting furnace cylinder was sealed with a flange, and water was injected into the main feed inlet. The water pressure was injected at a constant load rate (about 0.5h) to reach 0.6MPa. After maintaining the load for 1 hour, the pressure was slowly released to 0MPa (about 0.5h), and the strain operation trend and maximum value of the high-temperature strain gauge were recorded by the data acquisition instrument.
[0167] The strain value at the uniform base material is about 50 microstrain, the strain value at the heat affected zone is about 80 microstrain, and the strain value at the weld area is 40 microstrain; the water pressure is injected again, and after reaching 0.6MPa at a constant load rate (about 0.5h), the pressure is slowly released to 0MPa (about 0.5h) after maintaining the load for 1 hour, and the strain operation trend and maximum value of the high-temperature strain gauge are recorded by the data acquisition instrument. The strain value at the uniform base material is about 50 microstrain, the strain value at the weld is about 40 microstrain, and the strain value in the heat affected zone is about 100 microstrain; after 5 cycles, the strain value in the heat affected zone is maintained at about 120 microstrain and no longer increases, and the cyclic water pressure test is stopped.
[0168] The warping of the barrel caused by welding was almost flattened.
[0169] The fourth step is on-site high-temperature and pressure test operation. During the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, and air is introduced for heat circulation.
[0170] First, a high-temperature creep test of a standard welded joint specimen was carried out. The creep curve contains three stages, showing the percentage change of four creep strains over time. Among them, the rate reduction stage, the steady increase stage, and the accelerated increase stage. The recorded rate reduction stage time is about 220h, which is preliminarily determined to be the high-temperature pressure pre-operation time of the roasting furnace barrel.
[0171] The thermal strain and creep strain generated during the start-up of the key points of the roasting furnace were recorded by high-temperature strain gauges. The creep strain was small and the thermal strain was about 500 microstrain. During the high-temperature and pressurized pre-operation of the roasting furnace, it was started and stopped many times to record the thermal strain of the key points of the roasting furnace. When the start and stop reached 8 times, the difference between the microstrain before and after did not exceed 25 microstrain.
[0172] When the total running time reached 220h, the total strain curve of creep and thermal strain showed almost no increase, about 550 microstrain, then the operation was stopped and preparation for spraying began.
[0173] The fifth step is on-site spraying of tungsten carbide corrosion-resistant coating. When the roasting furnace is pre-operated and slowly cooled from the working temperature of 650℃ to 350℃, the inner wall of the roasting furnace is pre-sprayed by means of a long-pole spray gun. The long-pole spray gun is kept stationary, and the roasting furnace cylinder rotates at a constant speed through the movement of the bearing. The spraying thickness is about 320 microns. After one week of spraying, the long-pole spray gun moves forward a distance (about 5 cm).
[0174] After the roasting furnace is completely cooled, the final spraying of the inner wall of the roasting furnace is carried out, and the final coating thickness is inspected. The overall thickness of the coating is about 450 microns, and the error at each location does not exceed 15%.
[0175] After the roasting furnace ran for another cycle (three months), the inner wall was opened for inspection and it was found that the coating had not fallen off and the effect was good.
[0176] Example 6
[0177] A method for spraying a durable coating on the inner wall of a roasting furnace requires finishing and spraying the cylinder structure of a horizontal roasting furnace that has been used for a period of time. The specific method includes:
[0178] The first step is to eliminate the internal weld of the cylinder, remove the excess height, and eliminate protrusions.
[0179] An angle grinder is used with a 200-mesh shutter blade to grind the weld excess height of the inner wall of the roasting furnace to ensure that the surface has a certain degree of roughness. The shutter blade tangent direction is perpendicular to the weld direction until the weld and the parent material are in the same plane. In this way, the coating can be sprayed evenly inside the roasting furnace body, and the texture direction is perpendicular to the weld direction to avoid becoming a subsequent crack source.
[0180] Among them, for axial welds, the shutter blades swing back and forth along the circumferential direction for grinding; for circumferential welds, the shutter blades swing back and forth along the axial direction.
[0181] In the second step, a 1:1 solid model was established through ABAQUS simulation calculation software. The heat source was used for heating in the middle of the outside, forced convection and cavity radiation boundary conditions were imposed on the inner wall, and natural convection was carried out on the two ends of the outside with the outside world to carry out thermo-solid coupling analysis of the roasting furnace.
[0182] Roasting furnace shell size parameters:
[0183] Heating section 8000mm, insulation section 2×800mm, heating section thickness 300mm, non-insulation section 2×1000mm.
[0184] The inner diameter of the cylinder is 500mm, the outer diameter is 650mm, and the wall thickness is 30mm.
[0185] The heating section is 800℃, the cavity is radiant heat transfer, the radiation coefficient is 0.4, the heat loss caused by gas convection and materials is not considered, the insulation layer is glass fiber wool, the air convection coefficient is 0.005mW / mm2 / ℃, and the ambient temperature is 25℃.
[0186] Calculated load: thermal stress + internal pressure (0.6MPa) + gravity.
[0187] Since sequential coupling analysis is used, the heat transfer analysis unit type is DC3D8 and the stress analysis unit type is C3D8R.
[0188] The global layout is 60mm and the number of units in the thickness direction is 6.
[0189] Number of elements, 66156, number of nodes, 79681.
[0190] According to the results of literature research, the density, elastic modulus, Poisson's ratio, yield stress, thermal expansion coefficient, specific heat, and heat conduction parameters of N08810 material from room temperature to 1000°C were obtained.
[0191] For example, the material Incoloy 800HT has a density of 8g / cm3 and a thermal expansion coefficient of 15.0209×10-6 / ℃. The temperature variation curves of elastic modulus, yield stress, thermal expansion coefficient, specific heat, thermal conductivity, etc. can all be found.
[0192] The 1:1 solid model established by ABAQUS simulation software is subjected to mesh graphic analysis. A mesh transition is performed in the transition area from the heating section to the insulation section. The number of meshes in the thickness direction of the cylinder is not less than 6, and is set to 10 in this embodiment.
[0193] A fixed constraint is applied at one end of the cylinder to limit the rigid displacement, while preventing the constraint from being too large and affecting the calculation results of the concerned parts. The heat source, convection, thermal radiation, and changes in internal pressure are taken into account for the calculation.
[0194] Calculations show that the thermal stress in the transition area between the heat source and the exposed part is relatively large, reaching 60MPa.
[0195] At the same time, we carried out the baking furnace welding test plate 350*350*22mm 3 The simulation calculation of welding residual stress found that the residual stress of the weld and heat-affected zone was close to the yield stress value, and there was warping on both sides of the weld test plate, reaching 3°.
[0196] Therefore, the selection scheme for arranging high-temperature strain gauges at key points is as follows: select one weld on the outer wall of the roasting furnace, one heat-affected zone, one base material, and one temperature mutation site, and paste at least one strain gauge at each location.
[0197] Paste the high temperature strain gauge. The process includes:
[0198] First, use a thousand-blade grinder to grind the measured surface to remove surface burrs, rust layers and uneven pits. The grinding time is about 2 minutes.
[0199] Since the grinding speed of the lapis lathe is too fast, it is easy to cause the surface to overheat. Therefore, after the lapis lathe is ground, it is polished with 220-grit sandpaper, cleaned with anhydrous alcohol, coated with high-temperature ceramic glue, and heated and cured with a hot air gun. The curing temperature is controlled at about 600°C (greater than the equipment operating temperature of 500°C), the curing time is 5 hours, and the high-temperature strain gauge is pasted;
[0200] The high temperature ceramic glue is applied again to the area around the high temperature strain gauge and cured using a hot air gun at a curing temperature of 300°C for 3 hours.
[0201] The strain gauge transmits the electrical signal to the collector through the cable. The collector calculates the deformation of the key points of the roasting furnace through the change of the strain gauge resistance, and the unit is μ strain.
[0202] The third step is to carry out water pressure circulation experiments to strengthen the roasting furnace cylinder structure.
[0203] The maximum design pressure that the roasting furnace can withstand is 0.6MPa, and the operating pressure is generally 0.3MPa.
[0204] Under laboratory conditions, each outlet of the roasting furnace cylinder was sealed with a flange, and water was injected into the main feed inlet. The water pressure was injected at a constant load rate (about 0.5h) to reach 0.6MPa. After maintaining the load for 1 hour, the pressure was slowly released to 0MPa (about 0.5h), and the strain operation trend and maximum value of the high-temperature strain gauge were recorded by the data acquisition instrument.
[0205] The strain value at the uniform base material is about 50 microstrain, the strain value at the heat affected zone is about 80 microstrain, and the strain value at the weld area is 40 microstrain; the water pressure is injected again, and after reaching 0.6MPa at a constant load rate (about 0.5h), the pressure is slowly released to 0MPa (about 0.5h) after maintaining the load for 1 hour, and the strain operation trend and maximum value of the high-temperature strain gauge are recorded by the data acquisition instrument. The strain value at the uniform base material is about 50 microstrain, the strain value at the weld is about 40 microstrain, and the strain value in the heat affected zone is about 100 microstrain; after 5 cycles, the strain value in the heat affected zone is maintained at about 120 microstrain and no longer increases, and the cyclic water pressure test is stopped.
[0206] The warping of the barrel caused by welding was almost flattened.
[0207] The fourth step is on-site high-temperature and pressure test operation. During the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, and air is introduced for heat circulation.
[0208] The thermal strain and creep strain generated during the start-up of the key points of the roasting furnace were recorded by high-temperature strain gauges. The creep strain was small and the thermal strain was about 500 microstrain. During the high-temperature and pressurized pre-operation of the roasting furnace, it was started and stopped many times to record the thermal strain of the key points of the roasting furnace. When the start and stop reached 5 times, the difference between the microstrain before and after did not exceed 25 microstrain.
[0209] When the total running time reached 220h, the total strain curve of creep and thermal strain showed almost no increase, about 550 microstrain, then the operation was stopped and preparation for spraying began.
[0210] The fifth step is on-site spraying of tungsten carbide corrosion-resistant coating. When the roasting furnace is pre-operated and slowly cooled from the working temperature of 650℃ to 350℃, the inner wall of the roasting furnace is pre-sprayed by means of a long-pole spray gun. The long-pole spray gun is kept stationary, and the roasting furnace cylinder rotates at a constant speed through the movement of the bearing. The spraying thickness is about 320 microns. After one week of spraying, the long-pole spray gun moves forward a distance (about 5 cm).
[0211] After the roasting furnace is completely cooled, the final spraying of the inner wall of the roasting furnace is carried out, and the final coating thickness is inspected. The overall thickness of the coating is about 450 microns, and the error at each location does not exceed 18%.
[0212] After the roasting furnace ran for another cycle (three months), the inner wall was opened for inspection and it was found that the coating had not fallen off and the effect was good.
[0213] Other unmentioned places are the same as those in Example 1.
[0214] In the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. If the connection method is not specifically stated, conventional means such as bolts, rivets, welding, etc. in the prior art are used. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0215] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0216] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for spraying a durable coating on the inner wall of a roasting furnace, It is characterized in that The specific steps include: (1) Treat the inner wall of the roasting furnace to remove excess height and ensure surface roughness; (2) Determine the key points of stress and strain in the roasting furnace, paste high-temperature strain gauges at the key points, and arrange strain monitoring at the key points; (3) Set up a water pressure cycle experiment to determine the strain stability value; (4) Thermal stability cycle test under pressure to determine the minimum strain rate; (5) Corrosion-resistant coating spraying.
2. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that In the step (1), the specific method of surface treatment is to use an angle grinder with a 220-mesh louvered blade to grind the excess height of the weld on the inner wall of the roasting furnace.
3. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 2, It is characterized in that When grinding, the tangent direction of the louver blade is perpendicular to the direction of the weld until the weld and the base material are in the same plane.
4. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that In the step (2), the key stress and strain points of the roasting furnace are determined according to the method of thermo-solid coupling analysis of the roasting furnace.
5. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 4, It is characterized in that The thermo-solid coupling analysis method of the roasting furnace is to use ABAQUS simulation calculation software to perform finite element modeling and simulation on the roasting furnace cylinder structure, consider the influence of thermal stress, pressure and gravity on the force of the cylinder structure, and determine the key points of stress and strain of the roasting furnace.
6. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 5, It is characterized in that At least one high-temperature strain gauge is attached to each key stress and strain point of the roasting furnace, and each strain gauge transmits the electrical signal to the collector through a cable. The collector calculates the deformation of the key point of the roasting furnace through the change of the resistance of the strain gauge.
7. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that In the step (3), the specific method of the water pressure test is to seal each outlet of the roasting furnace cylinder with a flange, inject water into the feed inlet, and inject water pressure to reach the maximum design pressure that the roasting furnace can withstand at a constant load rate. After maintaining the load for 1 hour, slowly release the pressure to 0 MPa, and record the strain operation trend and maximum value of the high-temperature strain gauge through a data acquisition instrument; Water pressure was injected again to reach the maximum design pressure that the roasting furnace could withstand at a constant load rate. After maintaining the load for 1 hour, the pressure was slowly released to 0 MPa. The strain operation trend and maximum value of the high-temperature strain gauge were recorded by the data acquisition instrument.
8. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 7, It is characterized in that The water pressure cycle test is repeated until the strain trend of the high temperature strain gauge and the comparison of the maximum value before and after do not exceed 10%.
9. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that In the step (4), during the operation of the roasting furnace, the external heating device is turned on, the catalyst is not roasted in the roasting furnace, air is introduced for thermal circulation, and the creep test stress-strain curves of the roasting furnace body and the welded joint at a high temperature of 600° C. are determined by high-temperature strain gauges.
10. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 9, It is characterized in that The stress-strain curve is divided into three stages, in which the strain rate gradually decreases in the first stage, the strain rate is constant in the second stage, and the strain rate increases in the third stage.
11. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 10, It is characterized in that When the creep strain enters the second stage, the high-temperature and pressure pre-operation time of the roasting furnace shell is determined.
12. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 11, It is characterized in that During the pre-operation of the roasting furnace under high temperature and pressure, the furnace is started and stopped several times to record the thermal strain of key points of the roasting furnace. When the change in thermal strain generated by each start and stop and creep strain generated by high temperature and pressure does not exceed 10%, the operation is stopped.
13. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that In the step (5), spraying includes pre-spraying and final spraying.
14. A method for spraying a durable coating on the inner wall of a roasting furnace according to claim 1, It is characterized in that The pre-spraying is carried out by a long-pole spray gun on the inner wall of the roasting furnace after the roasting furnace is pre-run and slowly cooled from the working temperature of 600°C to 300°C; the final spraying is carried out by a long-pole spray gun on the inner wall of the roasting furnace after the roasting furnace is completely cooled.
Citation Information
Patent Citations
Response surface model-based roll coolant system technological parameter optimization method
CN105956326A
Phosphating or anodizing for improved bonding of thermal spray coating on engine cylinder bores
CN106282881A
Surface texture providing improved thermal spray adhesion
CN107523776A
Process method of reducing welding residual stress by using high-pressure water jet flow
CN109735695A
Method for eliminating welding residual stress based on high-pressure water-jet enhancing technology
CN109880988A
Cited By
Brake drum residual stress detection and shot blasting control parameter adaptive control method and system facing extreme temperature change environment
CN121069788A