Graphite tray cleaning method

By controlling the flow rate and concentration of the mixed halogen gas and carrier gas, combined with high-temperature hydrogen baking treatment, the graphite tray deposits are cleaned, solving the problem of incomplete cleaning in the prior art, extending the service life of the graphite tray and improving the quality of the wafer.

CN119016434APending Publication Date: 2024-11-26BEIJING ZHONGBOXIN SEMICON TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410975385.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing technologies struggle to completely remove deposits from graphite trays without damaging the silicon carbide coating, leading to shortened tray life, reduced wafer surface uniformity, and increased wafer cracking probability.

Method used

A mixture of halogen gas and carrier gas is used for pre-reaction and full reaction treatment, combined with high-temperature baking with hydrogen. The gas flow rate and concentration are controlled to avoid damage to the silicon carbide coating. The deposits are thoroughly cleaned through the sublimation and reduction reactions of halides.

Benefits of technology

It effectively extends the service life of graphite trays, improves the uniformity and reliability of wafer surfaces, and reduces manufacturing and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016434A_ABST
    Figure CN119016434A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite tray cleaning method. The graphite tray cleaning method comprises the following steps that preliminary cleaning is conducted; introducing a first mixed gas formed by mixing a halogen gas and a carrier gas, and carrying out pre-reaction treatment; introducing a second mixed gas formed by mixing a halogen gas and a carrier gas for full reaction treatment; hydrogen is introduced for high-temperature baking treatment; cooling to finish cleaning; wherein the molar ratio of the halogen gas to the carrier gas in the first mixed gas is smaller than that of the halogen gas to the carrier gas in the second mixed gas, and the gas flow of the first mixed gas is larger than that of the second mixed gas. According to the method, the repeated utilization rate of the graphite tray is greatly increased, and the service life of the graphite tray is prolonged; the halogen gas concentration and the gas flow of the first mixed gas and the second mixed gas are respectively controlled in a proper range, so that the silicon carbide coating can be prevented from being damaged while the sediments on the surface of the graphite tray are cleaned.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a graphite tray cleaning method. Background Art

[0002] In the development and manufacture of various semiconductor components such as light emitting diodes (LEDs), laser diodes (LDs), and electronic components including high-power, high-frequency, high-temperature transistors and integrated circuits, physical vapor deposition (PVD) equipment or chemical vapor deposition (CVD) equipment is often used to perform vapor phase epitaxial growth on a substrate. The substrate is mainly a graphite tray coated with a silicon carbide (SiC) coating to support the growth of thin single crystals.

[0003] As the growth material grows on the graphite tray for a long time, compound deposits are continuously deposited on the graphite tray, causing the thickness of the graphite tray to increase continuously. When the graphite tray is reused, the deposits on the edge of the substrate slot on the graphite tray grow too much, which can easily cause wafer surface contamination, affect the uniformity and optoelectronic parameters of the epitaxial wafer, and increase the probability of wafer cracking. At present, after the epitaxial growth is completed, the usual practice is to perform high-temperature cleaning on the graphite tray or manually scrape off the deposits to reduce the impact on the wafer growth parameters. The deposits are mainly group III compounds based on gallium nitride (GaN), aluminum nitride (AlN) and aluminum gallium nitride (AlGaN). The required reaction temperature is high and the film is dense. The above methods generally have problems such as incomplete cleaning, long processing time, easy damage to the tray or silicon carbide coating, and thus reducing the life of the graphite tray. Summary of the invention

[0004] The embodiment of the present application provides a graphite tray cleaning method, which is used to clean the surface deposits without damaging the tray body and the silicon carbide coating, thereby extending the service life of the graphite tray.

[0005] The embodiment of the present application provides a graphite tray cleaning method, comprising the following steps: preliminarily cleaning the deposits on the surface of the graphite tray; placing the graphite tray in a sealed chamber, introducing a first mixed gas of a halogen gas and a carrier gas for pre-reaction treatment; introducing a second mixed gas of a halogen gas and a carrier gas for full reaction treatment; introducing hydrogen (H2) for high-temperature baking treatment; controlling the temperature in the chamber to drop to room temperature to complete the cleaning; wherein the molar ratio of the halogen gas to the carrier gas in the first mixed gas is less than the molar ratio of the halogen gas to the carrier gas in the second mixed gas, and the gas flow rate of the first mixed gas is greater than the gas flow rate of the second mixed gas.

[0006] In the steps of the graphite tray cleaning method of the embodiment of the present application, the preliminary cleaning is a physical cleaning method, which is used to remove dust on the surface of the graphite tray and solid deposits that are not deeply engaged with the graphite tray. The pre-reaction treatment and the full reaction treatment can avoid damaging the silicon carbide coating while cleaning the deposits on the surface of the graphite tray by controlling the halogen gas concentration and gas flow rate of the first mixed gas and the second mixed gas in an appropriate range respectively. The hydrogen high-temperature baking treatment is used to accelerate the sublimation of halide solids by high temperature, increase the cleaning speed of the deposits, and hydrogen can react with the oxides in the silicon carbide coating to increase the purity of the silicon carbide. The graphite tray cleaning method can avoid damaging the silicon carbide coating while fully cleaning the deposits on the surface of the graphite tray, thereby extending the service life of the graphite tray.

[0007] In some exemplary embodiments, the halogen gas is chlorine (Cl2) and the carrier gas is nitrogen (N2). Chlorine is selected as the etching gas because it is easier to prepare and obtain. Nitrogen is selected as the carrier gas because it is cheaper and more economical than using rare gases such as argon and helium as the carrier gas.

[0008] In some exemplary embodiments, the molar ratio of chlorine to nitrogen in the first mixed gas is 1 / 10-1 / 8; the molar ratio of chlorine to nitrogen in the second mixed gas is 1 / 5-1 / 3.75. Within the above conditions, the molar fraction of chlorine in the first mixed gas is less than the molar fraction of chlorine in the second mixed gas. The first mixed gas has a low chlorine concentration, which can reduce corrosion to the silicon carbide coating. The second mixed gas has a high chlorine concentration, which can fully react with the deposits to achieve the purpose of removal.

[0009] In some exemplary embodiments, the gas flow rate of the first mixed gas is 4000sccm-6000sccm; the gas flow rate of the second mixed gas is 1000sccm-3000sccm. Within the above conditions, the gas flow rate of the first mixed gas is greater than the gas flow rate of the second mixed gas. The large gas flow rate of the first mixed gas can remove large particle deposits on the surface of the graphite tray by purging, and the small gas flow rate of the second mixed gas is more evenly distributed in the chamber and has a longer residence time, which is beneficial to the reaction of chlorine with deposits while reducing the corrosion caused to the silicon carbide coating.

[0010] In some exemplary embodiments, the temperature of the pre-reaction treatment is 650°C-750°C; the pressure of the pre-reaction treatment is 40torr-60torr; and the time of the pre-reaction treatment is 30min-40min. By controlling the temperature of the pre-reaction treatment within the range of 650°C-750°C, the chlorine gas can be fully activated and reacted, and the nitrogen gas only serves as a transport and purge. The pressure of the pre-reaction treatment is controlled between 40torr-60torr, so that the chlorine gas can be more accurately controlled at a lower pressure, the reaction atmosphere is cleaner, and it is more conducive to the uniform and rapid reaction of chlorine gas and sediments. The conversion of large-particle III-nitride deposits into III-halides takes about 30min-40min depending on the thickness of the deposits.

[0011] In some exemplary embodiments, the temperature of the full reaction treatment is 650°C-750°C; the pressure of the full reaction treatment is 70torr-80torr; and the time of the full reaction treatment is 30min-45min. Within the above conditions, the chlorine in the second mixed gas can fully and evenly react with the sediment, improve the sediment cleaning effect, and some sediments form dense films and bite deeply with the graphite tray. The full reaction treatment takes about 30min-45min.

[0012] In some exemplary embodiments, the gas flow rate of the hydrogen is 3000sccm-5000sccm; the pressure of the high temperature baking treatment is 0torr-50torr; the temperature of the high temperature baking treatment is 900℃-1100℃; and the time of the high temperature baking treatment is 3h-4h. If the baking temperature is too low or the baking time is too short, the deposits cannot be effectively removed; if the baking temperature is too high or the baking time is too long, the silicon carbide coating of the graphite tray will be damaged. Within the above conditions, hydrogen can fully react with the oxide layer that may be formed on the surface of the silicon carbide coating under appropriate gas flow conditions to improve the purity of silicon carbide; under appropriate temperature and baking time conditions, the deposits can be effectively removed while avoiding damage to the silicon carbide coating.

[0013] In some exemplary embodiments, during the pre-reaction treatment, the full reaction treatment and the high temperature baking treatment, the temperature in the chamber is controlled to be raised to the desired temperature at a heating rate of 20°C / min-30°C / min; after the high temperature baking treatment, the temperature in the chamber is controlled to be lowered to room temperature at a cooling rate of 20°C / min-30°C / min. This avoids the graphite tray from being broken due to too fast a heating / cooling rate, or long waiting time and unnecessary energy loss due to too slow a heating / cooling rate.

[0014] In some exemplary embodiments, the preliminary cleaning is any one of ultrasonic cleaning, high-pressure gas purging or dry ice purging, which can clean the dust on the surface of the graphite tray and the solid deposits that are not deeply bitten, in preparation for subsequent processing, without causing damage to the silicon carbide coating or the graphite tray body.

[0015] In some exemplary embodiments, the chamber is a reaction chamber of a MOCVD (metal organic chemical vapor deposition) device or a baking tray furnace. Both the MOCVD device and the baking tray furnace can provide a closed chamber, and can precisely control and monitor the gas source parameters (such as gas flow) and the parameters in the chamber (such as temperature, pressure, and processing time) to facilitate the cleaning step; there is no need to design or make equipment separately, which facilitates the implementation of the graphite tray cleaning method of the embodiment of the present application.

[0016] Based on the graphite tray cleaning method of the embodiment of the present application, the graphite tray is cleaned by the combined action of halogen gas corrosion and hydrogen high-temperature baking, and the cleaning effect is good. Among them, the gas flow rate of the first mixed gas is large and the halogen gas concentration is low. While blowing away the large-particle deposits on the surface of the graphite tray, the low halogen gas concentration can reduce the corrosion of the silicon carbide coating on the surface of the graphite tray; the gas flow rate of the second mixed gas is small and the halogen gas concentration is high. The halogen gas can react with the deposits evenly and fully, and the deposits are cleaned more thoroughly. At the same time, the small gas flow rate can reduce the corrosion caused to the silicon carbide coating. By controlling the halogen gas concentration and gas flow rate of the first mixed gas and the second mixed gas in an appropriate range, the deposits on the surface of the graphite tray can be cleaned while avoiding damage to the silicon carbide coating.

[0017] In addition, according to experimental data, without treating the surface of the graphite tray, the service life of the graphite tray is about 60 heats. By cleaning the graphite tray once every 30-40 heats, the total number of uses of the graphite tray can be increased to more than 400 heats, which greatly increases the reuse rate of the graphite tray, extends the service life of the graphite tray, and reduces the costs of graphite tray manufacturing, silicon carbide coating growth, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0019] Figure 1 The figure is a flow chart of a graphite tray cleaning method according to an embodiment of the present application. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0021] Embodiment 1

[0022] like Figure 1 As shown, it is a flow chart of the graphite tray cleaning method of some embodiments of the present application, please refer to Figure 1 The graphite tray cleaning method of the embodiment of the present application comprises the following steps:

[0023] Step 1: Perform preliminary cleaning of the deposits on the surface of the graphite tray by ultrasonic cleaning, high-pressure gas purging or dry ice purging.

[0024] The graphite tray to be cleaned is a graphite tray with a silicon carbide coating deposited on the surface. The surface deposits of the graphite tray are mainly group III nitrides, and the thickness of the deposits is related to the furnace number of the graphite tray. The initial cleaning is a physical method cleaning, which is used to remove dust on the surface of the graphite tray and solid deposits that are not deeply engaged with the graphite tray. Specifically, it can be one of ultrasonic cleaning, high-pressure gas purging or dry ice purging. Among them, ultrasonic cleaning can be carried out by an ultrasonic cleaning machine, and the cavitation, acceleration and straight flow of ultrasonic waves in the liquid are used to disperse and peel off the deposits to achieve the purpose of cleaning. At room temperature, use plasma water, acetone or other cleaning agents for ultrasonic cleaning for 10-30 minutes. High-pressure gas purging can be carried out through pipeline purging equipment, and high-flow gas is used to purge the surface deposits of the graphite tray to remove dust and impurities. Nitrogen or other inert gases can be used as gas. The gas source pressure is generally controlled between 0.6Mpa-0.8Mpa, the gas flow rate is greater than 20m / s, and the repeated purging time is 5min-10min. Dry ice purging can be performed using a dry ice cleaning machine. Dry ice particles are sprayed onto the surface of the graphite tray and the momentum change, sublimation and other energy conversion of the high-speed moving solid dry ice particles are utilized to quickly freeze the loose sediments, dust and impurities on the surface of the graphite tray, thereby condensing, catalyzing and peeling off. The dry ice consumption rate is about 500g / min and the repeated purging time is 10min-20min.

[0025] Step 2: Place the graphite tray in the chamber of the MOCVD equipment or the baking tray furnace, increase the temperature in the chamber to between 650°C and 750°C and maintain it stable, introduce a first mixed gas of chlorine and nitrogen for pre-reaction treatment, control the molar ratio of chlorine to nitrogen to between 1 / 10 and 1 / 8, control the gas flow rate of the first mixed gas to between 4000sccm and 6000sccm, control the pressure in the chamber to between 40torr and 60torr, and the pre-reaction treatment time to between 30min and 40min. After the pre-reaction treatment is completed, stop introducing the first mixed gas.

[0026] Step 3: introducing a second mixed gas of chlorine and nitrogen for full reaction treatment, controlling the molar ratio of chlorine to nitrogen to be between 1 / 5-1 / 3.75, controlling the gas flow rate of the second mixed gas to be between 1000sccm-3000sccm, controlling the pressure in the chamber to be between 70torr-80torr, and the full reaction treatment time to be 30min-45min. After the full reaction treatment is completed, stopping the introduction of the second mixed gas.

[0027] Specifically, the first mixed gas and the second mixed gas are used to react with the deposits to achieve the cleaning purpose. Both include halogen gas and carrier gas. The halogen gas, as a corrosive gas, can convert the group III nitride deposits into volatile group III halide solids. The carrier gas plays a role in transporting the halogen gas and controlling the flow of gas in and out of the chamber. The volatile group III halide solids can be carried out of the chamber under the continuous flow of the first mixed gas and the second mixed gas.

[0028] The corrosion rate of the halogen gas is related to the gas concentration and the gas flow rate. By controlling the halogen gas concentration and the gas flow rate of the first mixed gas and the second mixed gas respectively within an appropriate range, the deposits on the surface of the graphite tray can be cleaned while avoiding damage to the silicon carbide coating. In the graphite tray cleaning method of the embodiment of the present application, the molar ratio of the halogen gas to the carrier gas in the first mixed gas is less than the molar ratio of the halogen gas to the carrier gas in the second mixed gas, and the gas flow rate of the first mixed gas is greater than the gas flow rate of the second mixed gas. In this way, the gas flow rate of the first mixed gas is large, and the carrier gas purges the deposits while the halogen gas reacts with the deposits, which can remove large-particle deposits on the surface of the graphite tray, and pre-react with the deposits with deeper bites, paving the way for the subsequent full reaction and removal of the second mixed gas. The halogen gas concentration of the first mixed gas is low, which can reduce the corrosion of the silicon carbide coating on the surface of the graphite tray; the gas flow rate of the second mixed gas is small and the halogen gas concentration is high, so that the second mixed gas can be more evenly distributed in the chamber and have a longer residence time than the first mixed gas, and the halogen gas can react evenly and fully with the deposits with denser film formation and deeper bite, and the deposits are cleaned more thoroughly. At the same time, the second mixed gas with a small gas flow rate can reduce the corrosion of the silicon carbide coating on the surface of the graphite tray.

[0029] In the illustrated embodiment, chlorine is selected as the etching gas. Compared with the use of hydrogen chloride (HCl) gas, the ambient temperature required for chlorine as the etching gas is lower, which can reduce the energy loss of the cleaning process; compared with fluorine (F2), hydrogen iodide (HI) and other gases, chlorine is easier to prepare and obtain. Nitrogen is selected as the carrier gas. Compared with the use of rare gases such as argon and helium as carrier gases, nitrogen is cheaper and more economical. In one embodiment, chlorine can react with deposits such as gallium nitride and aluminum nitride to form metal chlorides such as gallium chloride (GaCl3) and aluminum chloride (AlCl3), so as to achieve the effect of removing surface deposits. The specific reaction equations are: 2AlN+3Cl2→2AlCl3+N2, 2GaN+3Cl2→2GaCl3+N2. Gallium chloride and aluminum chloride are both volatile at low pressure and can be carried out of the chamber under the continuous flow of the first mixed gas and the second mixed gas.

[0030] In terms of the selection of key parameters, chlorine has strong activity above about 600°C and can react quickly with sediments. Nitrogen, as a carrier gas, remains inert below about 800°C. By controlling the temperature of the pre-reaction treatment and the full reaction treatment within the range of 650-750°C, the chlorine can be fully activated and reacted, and the nitrogen only plays a role in purging and transportation. The pressure of the pre-reaction treatment is controlled between 40-60torr, so that chlorine can be more accurately controlled at a lower pressure, the reaction atmosphere is cleaner, turbulence is greatly reduced, the free path of molecules and the gas diffusion coefficient are increased, and it is more conducive to the uniform and rapid reaction of chlorine and sediments. The pressure of the full reaction treatment is controlled between 70-80torr, which is slightly larger than the pressure of the pre-reaction treatment, which is convenient for the second mixed gas to diffuse and distribute in the chamber and for the chlorine to fully react with the sediment. In one embodiment, it takes about 30-40 minutes to convert a large-grained Group III nitride deposit into a Group III halide depending on the thickness of the deposit, and it takes about 30-45 minutes to convert a Group III nitride deposit with a denser film and deeper engagement with the graphite tray into a Group III halide.

[0031] Step 4: At a rate of 30°C / s, continue to increase the temperature in the chamber to between 900°C and 1100°C and maintain this temperature, introduce hydrogen for high-temperature baking treatment, control the gas flow of hydrogen to 3000sccm-5000sccm, control the pressure in the chamber to be less than 40torr, and the high-temperature baking treatment time is 3h-4h. After the high-temperature baking treatment is completed, stop introducing hydrogen.

[0032] Part of the halide solid generated by the reaction between the sediment and the halogen gas volatilizes and flows out of the chamber with the first mixed gas or the second mixed gas, and the other part may remain on the surface of the graphite tray. The high-temperature baking treatment of hydrogen is used to accelerate the sublimation of the halide solid by high temperature, increase the cleaning speed of the sediment, and can act as a protective gas to prevent air from contacting the graphite tray. At the same time, an oxide layer may form on the surface of the silicon carbide coating, causing the surface of the graphite tray to lose its original performance and characteristics. Hydrogen, as a reducing agent, has a strong reducing property at high temperature. When hydrogen reacts with the oxide in the silicon carbide coating, the oxide is reduced to silicon carbide, thereby restoring the original performance of the graphite tray. The role of hydrogen is not only to reduce the oxide in the silicon carbide coating, but also to clean the surface impurities and organic matter, improve the purity of the graphite tray, and in addition, it can also improve the stability and reliability of the graphite tray by relaxing and reducing the stress inside the material.

[0033] During the hydrogen high-temperature baking process, if the baking temperature is too low or the baking time is too short, the deposits cannot be effectively removed; if the baking temperature is too high or the baking time is too long, the silicon carbide coating of the graphite tray will be damaged. Within the aforementioned conditions, hydrogen can fully react with the oxide layer that may be formed on the surface of the silicon carbide coating under appropriate gas flow conditions to improve the purity of silicon carbide; under appropriate temperature and baking time conditions, the deposits can be effectively removed while avoiding damage to the silicon carbide coating.

[0034] Step 5: Control the temperature in the chamber to drop to room temperature and complete the cleaning.

[0035] After the high-temperature hydrogen baking treatment, the sediment on the surface of the graphite tray is cleaned up, and the silicon carbide coating is purer. At this time, the temperature in the control chamber is slowly reduced to room temperature to complete the entire cleaning process. Take out the graphite tray and check the surface cleaning effect. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned and qualified graphite tray can be vacuum sealed for next use.

[0036] It should be noted that during the pre-reaction treatment, full reaction treatment and high temperature baking treatment, the temperature in the chamber needs to be controlled to rise to the required temperature at a heating rate of 20℃ / min-30℃ / min; after the high temperature baking treatment, the temperature in the chamber needs to be controlled to fall to room temperature at a cooling rate of 20℃ / min-30℃ / min. In this way, the graphite tray can be prevented from cracking due to too fast heating / cooling rate, or long waiting time and unnecessary energy loss due to too slow heating / cooling rate.

[0037] In addition, in the selection of reaction equipment, the pre-reaction treatment, full reaction treatment and hydrogen high-temperature baking treatment can be carried out in the reaction chamber of MOCVD equipment or a baking tray furnace, and the gas source parameters (such as gas flow) and chamber parameters (such as temperature, pressure, and treatment time) can be precisely controlled and monitored to facilitate the cleaning step. And there is no need to design or make equipment separately, which is convenient for the implementation of the graphite tray cleaning method of the embodiment of the present application.

[0038] According to experimental data, without treating the surface of the graphite tray, the service life of the graphite tray is about 60 heats; the graphite tray is cleaned once every 30-40 heats by the graphite tray cleaning method of the present application, which can increase the total number of uses of the graphite tray to more than 400 heats, greatly increasing the reuse rate of the graphite tray, extending the service life of the graphite tray, and reducing the costs of graphite tray manufacturing, silicon carbide coating growth, etc.

[0039] The graphite tray cleaning method of the present application will be further explained below in conjunction with specific embodiment parameters.

[0040] Embodiment 2:

[0041] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0042] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 700°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:9, the gas flow rate of the first mixed gas is controlled to be 5000sccm, the pressure in the chamber is controlled to be 50torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0043] A second mixed gas of chlorine and nitrogen is introduced for full reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:3, the gas flow rate of the second mixed gas is controlled to be 2000 sccm, the pressure in the chamber is controlled to be 75 torr, and the introduction of the second mixed gas is stopped after the full reaction treatment for 40 minutes;

[0044] At a rate of 30°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0045] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0046] Embodiment three:

[0047] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0048] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 700°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:10, the gas flow rate of the first mixed gas is controlled to be 6000sccm, the pressure in the chamber is controlled to be 60torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0049] A second mixed gas of chlorine and nitrogen is introduced for full reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:3, the gas flow rate of the second mixed gas is controlled to be 2000 sccm, the pressure in the chamber is controlled to be 75 torr, and the introduction of the second mixed gas is stopped after the full reaction treatment for 40 minutes;

[0050] At a rate of 30°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0051] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0052] Embodiment 4:

[0053] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0054] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 700°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:9, the gas flow rate of the first mixed gas is controlled to be 5000sccm, the pressure in the chamber is controlled to be 50torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0055] A second mixed gas of chlorine and nitrogen was introduced for full reaction treatment, the molar ratio of chlorine to nitrogen was controlled to be 1:5, the gas flow rate of the second mixed gas was controlled to be 3000 sccm, the pressure in the chamber was controlled to be 80 torr, and the introduction of the second mixed gas was stopped after full reaction treatment for 45 minutes;

[0056] At a rate of 30°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0057] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0058] Embodiment five:

[0059] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0060] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 700°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:8, the gas flow rate of the first mixed gas is controlled to be 4000sccm, the pressure in the chamber is controlled to be 40torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0061] A second mixed gas of chlorine and nitrogen is introduced for full reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:3, the gas flow rate of the second mixed gas is controlled to be 2000 sccm, the pressure in the chamber is controlled to be 75 torr, and the introduction of the second mixed gas is stopped after the full reaction treatment for 40 minutes;

[0062] At a rate of 30°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0063] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0064] Embodiment 6

[0065] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0066] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 700°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:9, the gas flow rate of the first mixed gas is controlled to be 5000sccm, the pressure in the chamber is controlled to be 50torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0067] A second mixed gas of chlorine and nitrogen was introduced for full reaction treatment, the molar ratio of chlorine to nitrogen was controlled to be 1:3.75, the gas flow rate of the second mixed gas was controlled to be 1000 sccm, the pressure in the chamber was controlled to be 70 torr, and the introduction of the second mixed gas was stopped after full reaction treatment for 40 minutes;

[0068] At a rate of 30°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0069] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0070] Embodiment 7

[0071] Place the graphite tray to be cleaned into the dry ice cleaning machine for dry ice purging, and control the cleaning time to 10 minutes;

[0072] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 750°C at a rate of 30°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:10, the gas flow rate of the first mixed gas is controlled to be 6000sccm, the pressure in the chamber is controlled to be 60torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 40 minutes;

[0073] A second mixed gas of chlorine and nitrogen was introduced for full reaction treatment, the molar ratio of chlorine to nitrogen was controlled to be 1:5, the gas flow rate of the second mixed gas was controlled to be 3000 sccm, the pressure in the chamber was controlled to be 80 torr, and the introduction of the second mixed gas was stopped after full reaction treatment for 45 minutes;

[0074] At a rate of 30°C / s, the temperature in the chamber was raised to 1100°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 5000sccm, and the pressure in the chamber was controlled to be 50torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0075] At a rate of 30°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0076] Embodiment 8

[0077] Place the graphite tray to be cleaned into the pipeline purge equipment for high-pressure gas purge, and control the cleaning time to 5 minutes;

[0078] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 650°C at a rate of 20°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:8, the gas flow rate of the first mixed gas is controlled to be 4000sccm, the pressure in the chamber is controlled to be 40torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 30 minutes;

[0079] A second mixed gas of chlorine and nitrogen was introduced for full reaction treatment, the molar ratio of chlorine to nitrogen was controlled to be 1:3.75, the gas flow rate of the second mixed gas was controlled to be 1000 sccm, the pressure in the chamber was controlled to be 70 torr, and the introduction of the second mixed gas was stopped after full reaction treatment for 30 minutes;

[0080] At a rate of 20°C / s, the temperature in the chamber was raised to 900°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 3000sccm, and the pressure in the chamber was controlled to be 10torr. After the high-temperature baking treatment for 3 hours, the introduction of hydrogen was stopped;

[0081] At a rate of 20℃ / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0082] Embodiment 9

[0083] Place the graphite tray to be cleaned in an ultrasonic cleaning machine for ultrasonic cleaning, and control the cleaning time to be 15 minutes at room temperature;

[0084] The graphite tray is placed in the chamber of the MOCVD equipment, the temperature in the chamber is raised to 750°C at a rate of 25°C / s and maintained at the temperature, a first mixed gas of chlorine and nitrogen is introduced for pre-reaction treatment, the molar ratio of chlorine to nitrogen is controlled to be 1:10, the gas flow rate of the first mixed gas is controlled to be 6000sccm, the pressure in the chamber is controlled to be 60torr, and the introduction of the first mixed gas is stopped after the pre-reaction treatment for 35 minutes;

[0085] A second mixed gas of chlorine and nitrogen was introduced for full reaction treatment, the molar ratio of chlorine to nitrogen was controlled to be 1:3.75, the gas flow rate of the second mixed gas was controlled to be 1000 sccm, the pressure in the chamber was controlled to be 70 torr, and the introduction of the second mixed gas was stopped after full reaction treatment for 30 minutes;

[0086] At a rate of 25°C / s, the temperature in the chamber was raised to 1000°C and maintained at this temperature, and hydrogen was introduced for high-temperature baking treatment. The gas flow rate of hydrogen was controlled to be 4000sccm, and the pressure in the chamber was controlled to be 40torr. After the high-temperature baking treatment for 4 hours, the introduction of hydrogen was stopped;

[0087] At a rate of 25°C / s, the temperature in the chamber is lowered to room temperature, the graphite tray is taken out, and the surface cleaning effect is checked. If the appearance is uniform and has no bumps, it can be basically judged that the cleaning is qualified. The cleaned graphite tray is vacuum sealed for use.

[0088] The same or similar numbers in the drawings of this embodiment correspond to the same or similar parts; in the description of this application, it should be understood that if the terms "upper", "lower", "left", "right", etc. indicate an orientation or position relationship based on the orientation or position relationship shown in the drawings, it is only for the convenience of describing this application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as a limitation on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.

[0089] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A graphite tray cleaning method, characterized in that: The following steps are involved: Carry out preliminary cleaning of the deposits on the surface of the graphite tray; The graphite tray is placed in a sealed chamber, and a first mixed gas of halogen gas and carrier gas is introduced to perform a pre-reaction treatment; A second mixed gas of halogen gas and carrier gas is introduced to perform a full reaction treatment; Passing hydrogen gas for high temperature baking treatment; Control the temperature in the chamber to drop to room temperature to complete the cleaning; The molar ratio of the halogen gas to the carrier gas in the first mixed gas is smaller than that in the second mixed gas, and the gas flow rate of the first mixed gas is greater than that of the second mixed gas.

2. The graphite tray cleaning method according to claim 1, characterized in that: The halogen gas is chlorine gas, and the carrier gas is nitrogen gas.

3. The graphite tray cleaning method according to claim 2, characterized in that: The molar ratio of chlorine to nitrogen in the first mixed gas is 1 / 10-1 / 8; the molar ratio of chlorine to nitrogen in the second mixed gas is 1 / 5-1 / 3.

75.

4. The graphite tray cleaning method according to claim 2, characterized in that: The gas flow rate of the first mixed gas is 4000 sccm-6000 sccm; the gas flow rate of the second mixed gas is 1000 sccm-3000 sccm.

5. The graphite tray cleaning method according to claim 2, characterized in that: The temperature of the pre-reaction treatment is 650°C-750°C; The pressure of the pre-reaction treatment is 40torr-60torr; The time of the pre-reaction treatment is 30min-40min.

6. The graphite tray cleaning method according to claim 2, characterized in that: The temperature of the full reaction treatment is 650°C-750°C; The pressure of the full reaction treatment is 70torr-80torr; The time for the sufficient reaction treatment is 30min-45min.

7. The graphite tray cleaning method according to claim 1, characterized in that: The gas flow rate of the hydrogen gas is 3000sccm-5000sccm; The pressure of the high temperature baking treatment is 0 torr-50 torr; The temperature of the high temperature baking treatment is 900°C-1100°C; The high temperature baking treatment time is 3h-4h.

8. The graphite tray cleaning method according to any one of claims 5 to 7, characterized in that: During the pre-reaction treatment, the full reaction treatment and the high-temperature baking treatment, the temperature in the chamber is controlled to rise to a desired temperature at a heating rate of 20°C / min-30°C / min; After the high temperature baking treatment is completed, the temperature in the chamber is controlled to cool down to room temperature at a cooling rate of 20° C. / min-30° C. / min.

9. The graphite tray cleaning method according to claim 1, characterized in that: The preliminary cleaning is any one of ultrasonic cleaning, high-pressure gas purging or dry ice purging.

10. The graphite tray cleaning method according to claim 1, characterized in that: The chamber is a reaction chamber of an MOCVD device or a baking tray furnace.

Citation Information

Patent Citations

  • Method for cleaning metal-organic chemical vapor deposition (MOCV) reaction chamber in situ

    CN102899636A

  • Reaction chamber, deposition device and cleaning method suitable for remote plasma cleaning

    CN111471980A

  • MOCVD equipment cleaning method

    CN111593327A

  • Method for quickly cleaning accumulated film in large-area vacuum chamber

    CN112609168A

  • Cleaning method of graphite disc

    CN113333374A