Method for extruding and processing weldless aluminum alloy round bar through biconical die
By heat treatment and scale peeling of 7000 series aluminum alloy rods and optimizing extrusion in double-conical molds, the internal weld problem of aluminum alloy profiles is solved, and the production of aluminum alloy round rods without welds is realized. Improves the mechanical and performance of the product.
Patent Information
- Application Number
- CN202411351077.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-26
AI Technical Summary
The aluminum alloy profile processed with existing continuous extrusion technology is prone to welds inside, which affects its mechanical properties and usage performance, resulting in a decrease in product yield.
The double-conical mold is used for extrusion processing. By heat treatment of the 7000 series aluminum alloy rod and peeling the surface oxide scale, combined with the optimized extrusion temperature and speed, welds are avoided.
The weldless properties of aluminum alloy round rods are realized, the mechanical properties and service performance of the product are improved, and the yield rate of the product is improved.
Smart Images

Figure CN119016532A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal processing, and in particular relates to a method for extruding a weld-free aluminum alloy round bar through a double-conical die. Background Art
[0002] Aluminum alloy has excellent electrical conductivity, thermal conductivity and corrosion resistance, and can be processed into various profiles for use in aircraft, new energy vehicles, mobile phones and other fields. At present, the demand for aluminum alloy profiles is gradually increasing, and the product quality requirements are getting higher and higher.
[0003] Aluminum alloy products processed by existing continuous extrusion technology have welds inside, and the welds will affect the mechanical properties and performance of the aluminum alloy material, and the yield of the processed aluminum alloy products will decrease. Summary of the invention
[0004] In order to solve the problem that the aluminum alloy profiles processed by the existing continuous extrusion technology have welds inside, the welds will affect the mechanical properties and performance of the aluminum alloy materials, and the yield of the processed aluminum alloy products decreases, the present invention provides a method for extruding aluminum alloy round bars without welds using a double-conical die.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A method for extruding a weld-free aluminum alloy round bar using a double-conical die comprises the following steps:
[0007] S1: taking a 7000 series aluminum alloy bar and placing it in a heating furnace for heat treatment to obtain a first aluminum alloy raw material;
[0008] S2: peeling off the oxide scale on the surface of the first aluminum alloy raw material to obtain a second aluminum alloy raw material;
[0009] S3: feeding the second aluminum alloy raw material into an extruder having a double-conical die for extrusion treatment to obtain an aluminum alloy round bar;
[0010] S4: Observe and determine whether there is a weld in the cross section of the aluminum alloy round bar through the set camera detection module. If there is a weld, it is determined to be an unqualified product; if there is no weld, it is determined to be a qualified product.
[0011] As a preferred technical solution of the present invention, in the step S1, 7000 series aluminum alloy raw material is put into a smelting furnace for smelting to obtain aluminum alloy melt, and the aluminum alloy melt is used to cast the 7000 series aluminum alloy rod.
[0012] As a preferred technical solution of the present invention, in the step S1, the heating furnace is controlled to heat treat the 7000 series aluminum alloy bar at a temperature of 400-450°C and a heat treatment time of 1-4 hours.
[0013] As a preferred technical solution of the present invention, in step S1, the heat treatment temperature of the heating furnace for the 7000 series aluminum alloy bar is set to 450°C, the heat treatment heating time is 1 hour, the heat treatment holding time is 2 hours, and after the heat treatment is completed, the first aluminum alloy raw material obtained is placed in the air to cool.
[0014] As a preferred technical solution of the present invention, in the step S2, the oxide scale peeling on the surface of the first aluminum alloy raw material is carried out at room temperature.
[0015] As a preferred technical solution of the present invention, in step S3, the extrusion temperature of the extruder on the second aluminum alloy raw material is controlled to be 400-480°C, the extrusion speed is 3-8rpm, and the diameter of the extruded aluminum alloy round bar is 9.5-27mm.
[0016] As a preferred technical solution of the present invention, in step S3, the extrusion temperature of the extruder for the second aluminum alloy raw material is set to 450°C, the extrusion speed is set to 4.5rpm, and the diameter of the extruded aluminum alloy round bar is 27mm.
[0017] As a preferred technical solution of the present invention, the 7000 series aluminum alloy rod contains at least one element among Al, Zn, Mg, Cu and trace elements such as Cr, Zr, Mn, Sc, Er, and Co.
[0018] As a preferred technical solution of the present invention, in step S3, the double-conical mold includes a feed port, a first conical cavity, a second conical cavity and a discharge port which are connected in sequence, the first conical cavity has a first inlet and a first outlet located at its axial ends, the second conical cavity has a second inlet and a second outlet located at its axial ends, the first inlet is connected to the feed port and has the same caliber as the feed port, the first outlet is connected to the second inlet and has the same caliber as the second inlet, the second outlet is connected to the discharge port and has the same caliber as the discharge port, the caliber of the first inlet is smaller than the caliber of the first outlet, and the caliber of the second inlet is larger than the caliber of the second outlet.
[0019] As a preferred technical solution of the present invention, the feed inlet, the first conical cavity, the second conical cavity, and the discharge port are coaxially arranged.
[0020] The beneficial effects of the present invention are:
[0021] The invention discloses a method for extruding a weld-free aluminum alloy round bar by using a double-cone die. The method comprises the following steps: heat treating a 7000 series aluminum alloy bar to make it suitable for subsequent extrusion, peeling off surface oxide scales to ensure that the surface of the raw material is clean and free of impurities during the subsequent extrusion process, and using a double-cone die for extrusion to optimize the extrusion path and force distribution, thereby avoiding the generation of welds during the extrusion process. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.
[0023] Figure 1 It is a schematic flow chart of a method for extruding a weld-free aluminum alloy round bar using a double-conical die according to the present invention;
[0024] Figure 2 A schematic diagram of the structure of a double-cone die for a method of extruding a weld-free aluminum alloy round bar using a double-cone die according to the present invention;
[0025] Figure 3 A cross-sectional view of an aluminum alloy round bar processed by a method for extruding an aluminum alloy round bar without weld seams using a double-conical die according to the present invention;
[0026] Description of main symbols
[0027] In the figure: 1, double-conical mold; 11, inlet; 12, first conical cavity; 13, second conical cavity; 14, outlet. DETAILED DESCRIPTION
[0028] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.
[0029] In the prior art, the process of producing aluminum alloy round bars by extrusion technology is prone to weld problems, which may reduce the overall strength, corrosion resistance and aesthetics of the material, and affect the performance and life of the product. Based on this, the inventors have proposed an improvement scheme that can effectively reduce or avoid the generation of welds in the production of aluminum alloy round bars, which is specifically described in the following embodiments.
[0030] See also Figure 1-3 This embodiment provides a method for extruding a weld-free aluminum alloy round bar using a double-conical die, comprising the following steps:
[0031] S1: taking a 7000 series aluminum alloy bar and placing it in a heating furnace for heat treatment to obtain a first aluminum alloy raw material;
[0032] S2: peeling off the oxide scale on the surface of the first aluminum alloy raw material to obtain a second aluminum alloy raw material;
[0033] S3: feeding the second aluminum alloy raw material into an extruder having a double-conical die 1 for extrusion treatment to obtain an aluminum alloy round bar;
[0034] S4: Observe and determine whether there is a weld in the cross section of the aluminum alloy round bar through the set camera detection module. If there is a weld, it is determined to be an unqualified product; if there is no weld, it is determined to be a qualified product.
[0035] In this embodiment, firstly, the microstructure of the 7000 series aluminum alloy bar is changed by heat treatment, such as grain growth, phase change, etc., so as to improve its processing performance and physical properties, so that it reaches a state suitable for extrusion, which is conducive to the smooth progress of the subsequent processing process. Subsequently, the oxide layer (i.e., oxide skin) on the surface of the first aluminum alloy raw material is removed to ensure the cleanliness of the extrusion surface, which helps to prevent the formation of welds caused by impurities during the extrusion process. Preferably, the oxide layer on the surface of the first aluminum alloy raw material can be scraped off by a lathe. Finally, the double-conical die 1 is used to optimize the material flow and stress state during the extrusion process, and reduce or eliminate the generation of welds. As described above, the operation process includes three main steps: heat treatment, oxide skin peeling, and double-conical die 1 extrusion. These steps are linked together to ensure the weld-free characteristics of the final product.
[0036] Further, in step S1, a 7000 series aluminum alloy raw material is put into a smelting furnace for smelting to obtain an aluminum alloy melt, and the aluminum alloy melt is used to cast a 7000 series aluminum alloy bar. It can be understood that in the production process of aluminum alloy products, the smelting and casting of raw materials are key initial steps. In this embodiment, the 7000 series aluminum alloy raw material is put into a smelting furnace for smelting, and is made into a bar through a casting process, in order to preliminarily remove impurities in the 7000 series aluminum alloy raw material and form a bar that is convenient for subsequent processing in an extruder.
[0037] Furthermore, in step S1, the heating furnace is controlled to heat treat the 7000 series aluminum alloy bar at a temperature of 400-450°C and a heat treatment time of 1-4 hours.
[0038] In one embodiment, the heat treatment temperature of the heating furnace for the 7000 series aluminum alloy rod is set to 450°C, the heat treatment heating time is 1 hour, the heat treatment holding time is 2 hours, and after the heat treatment is completed, the first aluminum alloy raw material is placed in the air to cool.
[0039] It is understandable that the 7000 series aluminum alloy rod is placed in a heating furnace, the heating rate is set to a certain value, and the temperature is raised to 450°C in about 1 hour. When the temperature reaches 450°C, the temperature is maintained for insulation treatment. The insulation time is 2 hours to allow the alloy elements to fully diffuse and redistribute to form an ideal phase structure and grain size. After the insulation is completed, the first aluminum alloy raw material is taken out of the heating furnace and placed in the air for natural cooling. Air cooling can avoid internal stress and structural defects caused by too fast cooling rate.
[0040] Further, in step S2, the oxide scale on the surface of the first aluminum alloy raw material is peeled off at room temperature. It is understandable that peeling off the oxide scale at room temperature can reduce the thermal impact on the aluminum alloy raw material, avoid changes or damage to material properties that may be caused by high-temperature treatment, and no additional heating or cooling equipment is required, thereby reducing energy consumption and production costs. After peeling off the oxide scale, the surface of the aluminum alloy raw material is smoother and cleaner, which is conducive to subsequent processing and use.
[0041] Furthermore, in step S3, the extrusion temperature of the extruder for the second aluminum alloy raw material is controlled to be 400-480°C, the extrusion speed is 3-8rpm, and the diameter of the extruded aluminum alloy round bar is 9.5-27mm.
[0042] In one embodiment, the extrusion temperature of the extruder for the second aluminum alloy raw material is set to 450°C, the extrusion speed is set to 4.5rpm, and the diameter of the extruded aluminum alloy round bar is 27mm. By accurately controlling the extrusion temperature, extrusion speed and forming size, it can be ensured that the aluminum alloy round bar has a smooth surface, accurate size, dense internal structure, and no defects such as cracks and inclusions.
[0043] Furthermore, the 7000 series aluminum alloy rod contains at least one element of Al, Zn, Mg, Cu and trace elements such as Cr, Zr, Mn, Sc, Er, and Co.
[0044] Furthermore, the double-conical mold 1 includes a feed port 11, a first conical cavity 12, a second conical cavity 13 and a discharge port 14 which are connected in sequence. The first conical cavity 12 has a first inlet and a first outlet located at its axial ends, and the second conical cavity 13 has a second inlet and a second outlet located at its axial ends. The first inlet is connected to the feed port 11 and has the same caliber as the feed port 11, the first outlet is connected to the second inlet and has the same caliber as the second inlet, the second outlet is connected to the discharge port 14 and has the same caliber as the discharge port 14, the caliber of the first inlet is smaller than the caliber of the first outlet, and the caliber of the second inlet is larger than the caliber of the second outlet. It can be understood that during the extrusion process, the aluminum alloy raw material enters the double-conical die 1 through the feed port 11, and first enters the first conical cavity 12. Since the first outlet diameter of the first conical cavity 12 is larger than the first inlet diameter, the aluminum material after entering the first conical cavity 12 from the feed port 11 will begin to disperse and be initially formed, that is, it flows outward along the side wall of the first conical cavity 12 from the first inlet until it fills the first outlet. Subsequently, the material will enter the second conical cavity 13 through the second inlet. Since the second outlet diameter of the second conical cavity 13 is smaller than the second inlet diameter, the aluminum material after entering the second conical cavity 13 from the second inlet will gradually gather and converge to the second outlet. Finally, the formed aluminum alloy round bar is extruded from the discharge port 14, so that the aluminum material can be uniformly compressed and shaped during the extrusion process, which helps to reduce internal stress and the generation of welds.
[0045] Specifically, the feed port 11, the first tapered cavity 12, the second tapered cavity 13, and the discharge port 14 are coaxially arranged. It can be understood that the coaxial arrangement of the feed port 11, the first tapered cavity 12, the second tapered cavity 13, and the discharge port 14 makes the extrusion force and friction force on the material in the mold more uniform, which helps to reduce the generation of internal stress and defects, and the straight and continuous flow path reduces the turbulence and eddy current phenomenon of the material in the mold, and improves the stability and precision of molding.
[0046] See also Figure 3 , Figure 3 The cross section of the aluminum alloy round bar produced by the inventive method of this solution shows that the cross section is smooth and has no cracks or welds. This observation directly reflects the effectiveness and superiority of the inventive method in the production of aluminum alloy round bars.
[0047] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for extruding a weld-free aluminum alloy round bar using a double-conical die, characterized in that: The following steps are involved: S1: taking a 7000 series aluminum alloy bar and placing it in a heating furnace for heat treatment to obtain a first aluminum alloy raw material; S2: peeling off the oxide scale on the surface of the first aluminum alloy raw material to obtain a second aluminum alloy raw material; S3: feeding the second aluminum alloy raw material into an extruder having a double-conical die for extrusion treatment to obtain an aluminum alloy round bar; S4: Observe and determine whether there is a weld in the cross section of the aluminum alloy round bar through the set camera detection module. If there is a weld, it is determined to be an unqualified product; if there is no weld, it is determined to be a qualified product.
2. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: In the step S1, a 7000 series aluminum alloy raw material is put into a smelting furnace for smelting to obtain an aluminum alloy melt, and the aluminum alloy melt is used to cast the 7000 series aluminum alloy rod.
3. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: In the step S1, the heating furnace is controlled to heat treat the 7000 series aluminum alloy bar at a temperature of 400-450° C. and a heat treatment time of 1-4 hours.
4. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 3, characterized in that: In the step S1, the heat treatment temperature of the heating furnace for the 7000 series aluminum alloy bar is set to 450°C, the heat treatment heating time is 1 hour, the heat treatment holding time is 2 hours, and after the heat treatment is completed, the first aluminum alloy raw material is placed in the air to cool.
5. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: In the step S2, the oxide scale on the surface of the first aluminum alloy raw material is peeled off at room temperature.
6. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: In step S3, the extrusion temperature of the extruder for the second aluminum alloy raw material is controlled to be 400-480° C., the extrusion speed is controlled to be 3-8 rpm, and the diameter of the aluminum alloy round bar formed by extrusion is controlled to be 9.5-27 mm.
7. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 6, characterized in that: In the step S3, the extrusion temperature of the extruder for the second aluminum alloy raw material is set to 450° C., the extrusion speed is set to 4.5 rpm, and the diameter of the aluminum alloy round bar formed by extrusion is set to 27 mm.
8. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: The 7000 series aluminum alloy bar contains at least one element among Al, Zn, Mg, Cu and trace elements such as Cr, Zr, Mn, Sc, Er, and Co.
9. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 1, characterized in that: In step S3, the double-conical mold includes a feed port, a first conical cavity, a second conical cavity and a discharge port which are connected in sequence, the first conical cavity has a first inlet and a first outlet located at two axial ends thereof, the second conical cavity has a second inlet and a second outlet located at two axial ends thereof, the first inlet is connected to the feed port and has the same caliber as the feed port, the first outlet is connected to the second inlet and has the same caliber as the second inlet, the second outlet is connected to the discharge port and has the same caliber as the discharge port, the caliber of the first inlet is smaller than the caliber of the first outlet, and the caliber of the second inlet is larger than the caliber of the second outlet.
10. The method for extruding a weld-free aluminum alloy round bar using a double-conical die according to claim 9, characterized in that: The feed inlet, the first conical cavity, the second conical cavity and the discharge port are coaxially arranged.
Citation Information
Patent Citations
Aluminum alloy roll bar production process suitable for cold heading production of parts
CN115673195A