Stepped cooling spinning forming method for fine-grain weak-texture titanium alloy thin-walled cylinder
By employing a stepped cooling spin forming method for thin-walled titanium alloy cylinders with fine grains and weak texture, the problems of coarse grains and strong anisotropy in the forming of thin-walled titanium alloy cylinders have been solved, enabling the manufacture of thin-walled titanium alloy cylinders with high thinning rate and high performance.
Patent Information
- Application Number
- CN202411224447.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Traditional titanium alloy thin-walled cylinder forming methods tend to result in coarse grains, strong anisotropy, and difficulty in forming thin-walled cylinders with large thinning rates, leading to poor overall mechanical properties of thin-walled cylinders.
A stepped cooling spin forming method for thin-walled cylinders of fine-grained, weakly textured titanium alloys is adopted. By pre-treating the billet, a lamellar structure with obvious β grain boundaries and regularly arranged α phases inside the grains is obtained. Combined with multi-pass heating spin forming, the forming temperature is gradually reduced. The microstructure is controlled by the coupling effect of temperature and deformation to achieve a fine-grained, weakly textured structure.
A thin-walled titanium alloy cylinder with a fine grain and weak texture, characterized by a large thinning rate, low anisotropy, and high strength and plasticity, was obtained, thus improving the overall mechanical properties of the material.
Smart Images

Figure CN119016580A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of titanium alloy thin-walled tube forming, and in particular to a step-cooling spinning forming method for a fine-grained weak-textured titanium alloy thin-walled tube. Background Art
[0002] With the rapid development of aerospace and other fields, the demand for high-performance, lightweight thin-walled parts is increasing. The use of lightweight high-strength materials and lightweight and efficient structures, combined with overall forming and manufacturing technology, is the main way to achieve this goal. Titanium alloy thin-walled cylindrical parts are an important and typical representative of this type, and their precise forming and manufacturing are of great significance to modern industrial needs.
[0003] The working environment of titanium alloy thin-walled tubes is complex, and they are often required to have a certain load-bearing capacity and uniform mechanical properties. Fine grains can usually significantly improve the strength and toughness of the alloy, while improving its fatigue performance; low texture strength can weaken the preferred orientation of the alloy and ensure the isotropy of the material. Therefore, it is very important to control the organization to obtain titanium alloy thin-walled tubes with fine grains, uniform organization, and low texture strength.
[0004] As an advanced loaded plastic forming process, spinning has the advantages of high process flexibility, simple mold structure, low forming load, and high production efficiency. It has become one of the most effective process methods for manufacturing large thin-walled rotating components. Traditional hot spinning of titanium alloy thin-walled tubes often uses forging preforms, which are mostly equiaxed. During the hot spinning process, the equiaxed grains of the forging are difficult to further refine, and the equiaxed grains show a certain preferential orientation and high-strength texture accompanied by spinning deformation. Therefore, the current titanium alloy thin-walled tube forming method has the problems of easy occurrence of coarse grains, strong anisotropy, difficulty in forming thin-walled tubes with large thinning rates, and poor comprehensive mechanical properties of thin-walled tubes. Summary of the invention
[0005] The embodiment of the present application provides a step-cooling spinning method for a fine-grained weak-textured titanium alloy thin-walled tube, which can solve the problems of the current titanium alloy thin-walled tube forming method being prone to coarse grains, strong anisotropy, difficulty in forming thin-walled tubes with large thinning rates, and poor comprehensive mechanical properties of thin-walled tubes.
[0006] In order to achieve the above-mentioned object, an embodiment of the present invention provides a step-cooling spinning method for a fine-grained weak-textured titanium alloy thin-walled tube, comprising:
[0007] The titanium alloy tube blank is subjected to a pretreatment process to obtain a titanium alloy prefabricated tube blank having a distinct β grain boundary and a lamellar structure with regularly arranged α phases inside the grains, and the titanium alloy prefabricated tube blank is subjected to a multi-pass heating spinning forming process to obtain a fine-grained weak-textured titanium alloy thin-walled tube;
[0008] The blank pretreatment includes: the titanium alloy tube blank is rapidly heated to a temperature 15°C to 35°C above the phase transition point of the titanium alloy for a first preset time, and then rapidly cooled at a preset cooling rate after short-term heat preservation for a second preset time;
[0009] The heating spinning step comprises: rapidly heating the titanium alloy preformed tube blank to a preset forming temperature and then spinning, each pass is rapidly heated to the preset forming temperature and the wall thickness reduction rate is not less than a first percentage, and the spinning is terminated when the total thinning rate is higher than a second percentage, and the titanium alloy thin-walled tube after spinning is air-cooled on the core mold to a preset temperature and then demolded;
[0010] The preset forming temperature of each pass is in a two-phase region higher than the recrystallization temperature and gradually decreases with the increase of the number of heating times.
[0011] In a possible implementation, the preset forming temperature reached in each heating pass is reduced in a step-by-step manner as the number of heating times increases.
[0012] In a possible implementation, the first preset time does not exceed 10 minutes.
[0013] In a possible implementation, the second preset time is 1 min to 2 min.
[0014] In a possible implementation, the preset cooling rate is 130° C. / min to 230° C. / min.
[0015] In a possible implementation, the first percentage is 20%, and the second percentage is 80%.
[0016] In a possible implementation, the preset temperature is 350°C to 400°C.
[0017] A step-cooling spinning forming method for a fine-grained weak-textured titanium alloy thin-walled tube provided in an embodiment of the present invention has at least the following technical effects or advantages:
[0018] The step-cooling spinning forming method of the fine-grained weak-textured titanium alloy thin-walled tube of the embodiment of the present application is to pre-treat the titanium alloy tube blank to obtain a titanium alloy prefabricated tube blank with obvious β grain boundaries and regularly arranged α phases inside the grains, and then perform multiple heating spinning forming steps on the titanium alloy prefabricated tube blank to obtain a fine-grained weak-textured titanium alloy thin-walled tube. The pre-treating of the blank includes: the titanium alloy tube blank is rapidly heated to a temperature greater than 15°C to 35°C of the phase transition point of the titanium alloy after a first preset time, so that it reaches the β single-phase region, and then is rapidly cooled at a preset cooling rate after a short-term heat preservation for a second preset time. The heating spinning forming step includes: the titanium alloy prefabricated tube blank is rapidly heated to a preset forming temperature and then spin-formed, each pass is rapidly heated to the preset forming temperature and the wall thickness thinning rate is not less than the first percentage, and the spinning is terminated when the total thinning rate is higher than the second percentage. After the spinning is completed, the titanium alloy thin-walled tube is air-cooled to a preset temperature on the core mold and then demolded. The preset forming temperature of each pass is in the two-phase region higher than the recrystallization temperature and gradually decreases with the increase of the number of heating times. The preset forming temperature is step-wise reduced to the two-phase region for subsequent multiple-pass spinning forming. This is a step-cooling heating spinning forming process, which makes the titanium alloy tube preform undergo rapid heating, multiple large deformations, and rapid cooling. The organization is regulated by the coupling effect of temperature and deformation to obtain a fine-grained weak-textured titanium alloy thin-walled tube with a large thinning rate, weak anisotropy, high strength and plasticity, and good comprehensive mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0020] Figure 1 Physical diagram of components provided for specific embodiments of the present application;
[0021] Figure 2 A cross-sectional view of a component transition zone provided for a specific embodiment of the present application;
[0022] Figure 3 The microstructure diagram (a) of the RD-ND cross section of the titanium alloy tube blank provided in the embodiment of the present application (low magnification on the left, high magnification on the right) and the microstructure diagram (b) of the RD-ND cross section of a specific embodiment of the present application (low magnification on the left, high magnification on the right);
[0023] Figure 4 The secondary inverse pole figure (a) of the titanium alloy tube blank provided in the embodiment of the present application and the secondary inverse pole figure (b) of the fine-grained weak-textured titanium alloy thin-walled tube in the specific embodiment of the present application;
[0024] Figure 5 It is a pole figure of the {0001} pole of the fine-grained weakly textured titanium alloy thin-walled tube of a specific embodiment of the present application;
[0025] Figure 6 The microstructure diagrams of the NR cross-sectional areas at different axial positions of the fine-grained weak-textured titanium alloy thin-walled tube of the specific embodiment of the present application are as follows: (a) is the NR cross-sectional area near the cycloid end, and (b) is the NR cross-sectional area far from the cycloid end;
[0026] Figure 7 The microstructure diagrams of different regions in the thickness direction of the fine-grained weak-textured titanium alloy thin-walled tube provided in the embodiment of the present application, (a1) is the outer surface region, (a2) is the central region, and (a3) is the inner surface region;
[0027] Figure 8 The tensile stress-strain curve of a thin-walled tube of a fine-grained weakly textured titanium alloy of a specific embodiment;
[0028] Fig. 9 The fracture morphology of a fine-grained weakly textured titanium alloy thin-walled tube according to a specific embodiment. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The embodiment of the present invention provides a step-cooling spinning method for a fine-grained weak-textured titanium alloy thin-walled tube, comprising:
[0031] The titanium alloy tube blank is pretreated to obtain a titanium alloy preformed tube blank with obvious β grain boundaries and regularly arranged α phase lamellar structure inside the grains, and then the titanium alloy preformed tube blank is subjected to multiple heating and spinning forming steps to obtain a fine-grained weak-textured titanium alloy thin-walled tube.
[0032] The pretreatment of the blank includes: the titanium alloy tube blank is rapidly heated to a temperature greater than the phase transformation point of the titanium alloy by 15°C to 35°C (which can be a typical but non-limiting temperature such as 15°C, 20°C, 25°C, 30°C and 35°C) for a first preset time, and then rapidly cooled by a preset cooling rate after a short-term heat preservation for a second preset time. Among them, the first preset time does not exceed 10 minutes, and can be a typical but non-limiting temperature such as 1min, 2min, 3min, 4min, 5min, 6min, 7min, 8min and 9min. The second preset time is 1min to 2min, which can be a typical but non-limiting time such as 1min, 1.5min and 2min. The preset cooling rate is 130℃ / min to 230℃ / min, which can be typical but non-limiting rates such as 130℃ / min, 140℃ / min, 150℃ / min, 160℃ / min, 170℃ / min, 180℃ / min, 190℃ / min, 200℃ / min, 210℃ / min, 220℃ / min and 230℃ / min.
[0033] The heating spinning forming step includes: rapidly heating the titanium alloy preformed tube blank to a preset forming temperature and then spinning it, each pass is heated to the preset forming temperature by rapid heating and the wall thickness reduction rate is not less than a first percentage, and the spinning is terminated when the total thinning rate is higher than a second percentage. After the spinning is completed, the titanium alloy thin-walled tube is air-cooled on the core mold to a preset temperature and then demolded.
[0034] The first percentage is 20%, and the second percentage is 80%, so that a titanium alloy thin-walled tube with good organizational properties can be obtained. The preset temperature is 350°C to 400°C, and can be typical but non-limiting temperatures such as 350°C, 360°C, 370°C, 380°C, 390°C and 400°C.
[0035] The preset forming temperature of each pass is in the two-phase region above the recrystallization temperature and gradually decreases with the increase of heating times.
[0036] Furthermore, the preset forming temperature of each heating pass is reduced in steps as the number of heating times increases, thereby saving energy. At the same time, the titanium alloy tube blank undergoes processes such as rapid heating, multiple large deformations, and rapid cooling, ensuring that the forming temperature of each pass is in the two-phase region. Each spinning pass changes the preset forming temperature, thereby better utilizing the coupling effect of temperature and deformation.
[0037] The step-cooling spinning forming method of the fine-grained weak-textured titanium alloy thin-walled tube of the embodiment of the present application is to pre-treat the titanium alloy tube blank to obtain a titanium alloy prefabricated tube blank with obvious β grain boundaries and regularly arranged α phases inside the grains, and then perform multiple heating spinning forming steps on the titanium alloy prefabricated tube blank to obtain a fine-grained weak-textured titanium alloy thin-walled tube. The pre-treating of the blank includes: the titanium alloy tube blank is rapidly heated to a temperature greater than 15°C to 35°C of the phase transition point of the titanium alloy after a first preset time, so that it reaches the β single-phase region, and then is rapidly cooled at a preset cooling rate after a short-term heat preservation for a second preset time. The heating spinning forming step includes: the titanium alloy prefabricated tube blank is rapidly heated to a preset forming temperature and then spin-formed, each pass is rapidly heated to the preset forming temperature and the wall thickness thinning rate is not less than the first percentage, and the spinning is terminated when the total thinning rate is higher than the second percentage. After the spinning is completed, the titanium alloy thin-walled tube is air-cooled to a preset temperature on the core mold and then demolded. The preset forming temperature of each pass is in the two-phase region higher than the recrystallization temperature and gradually decreases with the increase of the number of heating times. The preset forming temperature is step-wise reduced to the two-phase region for subsequent multiple-pass spinning forming. This is a step-cooling heating spinning forming process, which makes the titanium alloy tube preform undergo rapid heating, multiple large deformations, and rapid cooling. The organization is regulated by the coupling effect of temperature and deformation to obtain a fine-grained weak-textured titanium alloy thin-walled tube with a large thinning rate, weak anisotropy, high strength and plasticity, and good comprehensive mechanical properties.
[0038] The advantages of step cooling are: the plasticity of titanium alloy decreases significantly with increasing temperature, so deformation at high temperature can increase the deformation amount, and effective thinning of the tube blank can be achieved with fewer spinning passes. Secondly, deformation at high temperature, especially above the phase transition temperature, can effectively change the structure of the material, but since the grains obtained at high temperature are relatively coarse, it will have an adverse effect on the performance. Therefore, the temperature is gradually lowered during the subsequent spinning process to achieve the purpose of organizational regulation, so that the material can be deformed at a lower temperature to refine the grains and improve the performance. Finally, the heating rate during the heating of the blank is increased, and the blank is quickly cooled in the air after the forming is completed. The material is quickly cooled after large deformation by multiple step cooling passes, which can effectively regulate the material structure during the spinning process, obtain the structural characteristics of fine grains and weak textures, and thus maintain good structural integrity and performance.
[0039] Specifically, after pretreatment of the titanium alloy tube blank, the temperature, deformation amount, speed and other parameters during the step cooling spinning process can be controlled to achieve grain refinement and texture control, thereby obtaining a fine-grained, weak-textured titanium alloy thin-walled tube with a large thinning rate and high performance.
[0040] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, and to significantly reflect the progressiveness of the titanium alloy thin-walled tube forming method of the embodiment of the present application, the above technical scheme is illustrated by the following specific embodiments.
[0041] The titanium alloy barrel blank in this experiment is a TC4 titanium alloy barrel part, and the measured composition mass percentage (%) of the material is: 6.14Al, 4.13V, 0.16Fe, 0.016C, 0.014N, 0.09O, and the rest is Ti. The inner diameter of the titanium alloy barrel blank is 158mm, and the wall thickness is 14mm. The embodiment of the present application adopts a positive spinning process, with a roller diameter of 250mm, a roller height of 50mm, a roller fillet radius of 10mm, a roller forming angle of 22.5°, a roller exit angle of 27.5°, a core mold speed of 60r / min, and a feed ratio of 1.0mm / s. Specific embodiments
[0043] The titanium alloy barrel blank is subjected to a blank pretreatment to obtain a titanium alloy prefabricated barrel blank having a distinct β grain boundary and a lamellar structure with regular arrangement of α phase inside the grains. Specifically, the titanium alloy barrel blank is rapidly heated to 1000°C (15°C to 35°C higher than the phase transition point temperature of the titanium alloy, and the TC4 phase transition point temperature is 970°C) for 8 minutes, and then rapidly cooled at 130°C / min after a short-term heat preservation for 1 minute to obtain a titanium alloy prefabricated barrel blank having a distinct β grain boundary and a lamellar structure with regular arrangement of α phase inside the grains.
[0044] The titanium alloy preformed tube blank was rapidly heated to 970°C and then subjected to the first spinning process, with a wall thickness reduction of 3 mm and a wall thickness reduction rate of 21.4%.
[0045] The titanium alloy preformed tube blank was rapidly heated to 950°C and then subjected to a second spinning process, with a wall thickness reduction of 3 mm and a wall thickness reduction rate of 27.3%.
[0046] The titanium alloy preformed tube blank is rapidly heated to 900° C. and then subjected to a third spinning process, with a wall thickness reduction of 2 mm and a wall thickness reduction rate of 25%.
[0047] The titanium alloy preformed tube blank was rapidly heated to 850°C and then subjected to the fourth spinning process, with a wall thickness reduction of 2 mm and a wall thickness reduction rate of 33.3%.
[0048] The titanium alloy preformed tube blank is rapidly heated to 830° C. (TC4 recrystallization temperature is 750° C.) and then subjected to the fifth spinning process, with a wall thickness reduction of 2 mm and a wall thickness reduction rate of 50%.
[0049] The total thinning rate is 85.7%. After spinning, the titanium alloy thin-walled tube is air-cooled to 400°C on the core mold and then demolded to obtain a fine-grained weak-textured titanium alloy thin-walled tube. The grain size is about 2μm to 3μm, the texture strength is about 1.8, the tensile strength can reach 1250MPa, and the elongation can reach 8%.
[0050] Rapid heating uses induction heating, and its average heating efficiency is approximately 1.8℃ / s~2.1℃ / s.
[0051] Figure 1 A physical diagram of components provided for a specific embodiment of the present application.
[0052] Figure 2 This is a cross-sectional view of the transition zone of a component provided in a specific embodiment of the present application. From the figure, it can be intuitively seen that the component has undergone five passes of spinning deformation, and its wall thickness gradually decreases. Finally, the wall thickness is effectively thinned.
[0053] Figure 3 The microstructure diagram (a) of the RD-ND cross section of the titanium alloy tube blank provided in the embodiment of the present application (low magnification on the left, high magnification on the right) and the microstructure diagram (b) of the RD-ND cross section of the specific embodiment of the present application (low magnification on the left, high magnification on the right). Figure 3 As shown in (a), the equiaxed grains in the TC4 titanium alloy tube blank are relatively large and unevenly distributed. Figure 3 As shown in (b), the organizational morphology of the component has undergone a major transformation. At this time, after the component is spun, the lamellar structure of the prefabricated tube blank is destroyed, forming a hemispherical structure. At this time, lamellar grains can no longer be observed in the organization, and instead, lath grains and spheroidized equiaxed grains are interwoven, forming a hemispherical organization of lath grains and spheroidized grains. With the increase in deformation, the proportion of spheroidized grains gradually increases, and the lath grains after five spinning passes are basically completely spherical. At the same time, as the deformation continues to increase, the equiaxed grains after spheroidization undergo more serious distortion in the subsequent deformation process, and the grains are elongated along the RD direction. After five spinning passes, the grain length direction is about 8μ~10μm, and the width direction is about 2μ~3μm.
[0054] By adopting the titanium alloy thin-walled tube forming method of the embodiment of the present application, the titanium alloy tube blank is transformed from coarse equiaxed grains to lamellar grains and then to spheroidized grains, which is refined, thereby improving the comprehensive performance of the formed titanium alloy thin-walled tube.
[0055] Figure 4 The secondary inverse pole figure (a) of the titanium alloy tube blank provided in the embodiment of the present application and the secondary inverse pole figure (b) of the fine-grained weakly textured titanium alloy thin-walled tube provided in the specific embodiment of the present application. It can be found that when no deformation occurs, the crystal orientation of the grains is basically randomly distributed, and the orientation of some grains is <1010> and <1120> The crystal orientation is biased towards the ND direction, such as Figure 4 (a) As shown. After the fifth spinning pass, the lamellar grains inside the material have been basically spheroidized. At this time, the newly spheroidized grains have no obvious preferred orientation. It can be observed that the grain size is small and there are grains in all directions. <0001> Direction and There are more grains with directions parallel to the ND direction, e.g. Figure 4(b) This phenomenon shows that as the spinning process proceeds, the spheroidization of the lamellar layer is beneficial to weakening the texture of the material and improving the uniformity of the material's organization.
[0056] Figure 5 This is the pole figure of the {0001} pole of the fine-grained weak-textured titanium alloy thin-walled tube of the specific embodiment of the present application. After five spinning deformations, the c-axis of the grain has been rotated to be basically parallel to the ND direction, and the texture strength of the tube has been significantly reduced. This is because during the spinning process of the lamellar structure, the α phase and the c-axis will first deflect in the RD direction, and then deflect in the ND direction through the action of spinning. Together with the shear deformation, the texture strength of the spinning tube is significantly reduced.
[0057] Figure 6 The microstructure diagrams of the NR cross-section areas at different axial positions of the fine-grained weakly textured titanium alloy thin-walled tube of the specific embodiment of the present application are as follows: (a) is the NR cross-section area near the cycloid end, and (b) is the NR cross-section area far from the cycloid end. As can be seen from the figure, the organizational differences at different cross-section positions in the RD direction are not large, and the organizational morphology is basically the same, ensuring the organizational uniformity in the RD direction.
[0058] Figure 7 The microstructure diagram of different regions of the thin-walled titanium alloy tube with fine grain and weak texture in the thickness direction of the embodiment of the present application is shown in the figure. As can be seen from the figure, the structure of the finally formed thin-walled titanium alloy tube is relatively uniform along the thickness direction, and the structure of the inner and outer surfaces and the central area is basically unchanged, ensuring the uniformity of the structure in the thickness direction.
[0059] Figure 8 The tensile stress-strain curve of the fine-grained weak-textured titanium alloy thin-walled tube of the specific embodiment is shown in Figure 1. After five passes of spinning, the elongation of the component can reach 7.2%, and its plasticity is basically the same as that of the initial titanium alloy tube blank, but the strength is significantly improved by about 30% compared with the initial titanium alloy tube blank.
[0060] Fig. 9 The fracture morphology of a fine-grained weak-textured titanium alloy thin-walled tube in a specific embodiment. After five spinning passes, the plasticity of the titanium alloy thin-walled tube does not change much, and the fracture presents an obvious ductile fracture with a 45° inclination, which is an obvious ductile fracture feature. A large number of dimples can be observed, and they are evenly distributed.
[0061] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other. Each embodiment focuses on the differences from other embodiments.
[0062] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the present application.
Claims
1. A step-cooling spinning method for a thin-walled tube of a fine-grained weak-textured titanium alloy, characterized in that: include: The titanium alloy tube blank is subjected to a pretreatment process to obtain a titanium alloy prefabricated tube blank having a distinct β grain boundary and a lamellar structure with regularly arranged α phases inside the grains, and the titanium alloy prefabricated tube blank is subjected to a multi-pass heating spinning forming process to obtain a fine-grained weak-textured titanium alloy thin-walled tube; The blank pretreatment includes: the titanium alloy tube blank is rapidly heated to a temperature 15°C to 35°C above the phase transition point of the titanium alloy for a first preset time, and then rapidly cooled at a preset cooling rate after short-term heat preservation for a second preset time; The heating spinning step comprises: rapidly heating the titanium alloy preformed tube blank to a preset forming temperature and then spinning, each pass is rapidly heated to the preset forming temperature and the wall thickness reduction rate is not less than a first percentage, and the spinning is terminated when the total thinning rate is higher than a second percentage, and the titanium alloy thin-walled tube after spinning is air-cooled on the core mold to a preset temperature and then demolded; The preset forming temperature of each pass is in a two-phase region higher than the recrystallization temperature and gradually decreases with the increase of the number of heating times.
2. The step-cooling spinning forming method for a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The preset forming temperature reached by each heating pass is reduced step by step as the number of heating times increases.
3. The step-cooling spinning forming method of a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The first preset time does not exceed 10 minutes.
4. The step-cooling spinning forming method of a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The second preset time is 1 minute to 2 minutes.
5. The step-cooling spinning forming method of a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The preset cooling rate is 130° C. / min to 230° C. / min.
6. The step-cooling spinning forming method of a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The first percentage is 20%, and the second percentage is 80%.
7. The step-cooling spinning forming method of a fine-grained weak-textured titanium alloy thin-walled tube according to claim 1 is characterized in that: The preset temperature is 350°C to 400°C.
Citation Information
Patent Citations
Method for manufacturing pure titanium tube by welding and spinning rolling plate
CN103121047A
Cross-phase region forging process of TC18 titanium alloy on screw press
CN104480416A
Preparation method for large-diameter thick-wall seamless titanium alloy barrel
CN106944494A
Forming and processing method of titanium alloy high-pressure seamless gas cylinder for ships
CN112246947A
Cold spinning forming method for large-diameter titanium alloy cylindrical part
CN114160653A