Forging method for producing large-diameter solid forge piece through continuous casting billet and solid forge piece
By using upper and lower cylinder V-shaped anvil pressing jaws and upsetting components for material separation and upsetting processes in continuous casting blank production, the problem of poor compaction effect of the center of the large-diameter solid forging blank is solved, and a good blank is achieved Compacting and defect reduction.
Patent Information
- Application Number
- CN202411304533.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
AI Technical Summary
In the process of producing large-diameter solid forgings in continuous casting billets, the compaction effect of the center of the billet is poor, resulting in serious ultrasonic flaw detection defects.
The upper and lower cylinder V-shaped anvils are used to press the jaws on the axial intermediate area of the columnar continuous casting billet to form a jaw segment and divide it axially in the jaw segment. The upsetting and drawing process is used to control the pressure The reduction rate is between 20-35%, to ensure good compaction effect of the center of the blank.
Through the above method, the lateral widening of the blank is effectively limited, ensuring that the center of the blank is in a three-way compressive stress state, improving the hydrostatic pressure and strain distribution, preventing gas from entering the blank, significantly improving the compaction effect of the blank, and avoiding ultrasonic flaw detection defects.
Smart Images

Figure CN119016652A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forging, and in particular to a forging method for producing a large-diameter solid forging from a continuous casting billet and the solid forging. Background Art
[0002] At present, continuous casting billets are mostly used to produce small-diameter solid forging products. In traditional manufacturing, large-diameter (>1000mm) solid forgings are mostly forged by die-cast steel ingots, and the shrinkage holes, looseness and other defects in the center of the steel ingot are compacted through upsetting, drawing and other processes; however, the production of forgings by die-cast steel ingots has problems such as water riser discards, high fire consumption, and long production cycle, which affect production efficiency and cost. The production of forgings by continuous casting billets can achieve multiple pieces from one out, but the continuous casting billet needs to be divided into multiple billets for upsetting and drawing processes. In the production process, if direct heating gas cutting, mechanical processing and other material separation methods are used, the defects in the center of the continuous casting billet will be directly exposed to the air, causing gas to enter the center of the billet. Since the gas is equivalent to foreign matter for the billet, the gas cannot be deformed and cannot be discharged during the forging process, resulting in poor compaction of the center of the billet, so that the ultrasonic flaw detection defects of the large-diameter solid forgings obtained in the end exceed the standard seriously. Summary of the invention
[0003] The problem solved by the invention is that during the process of producing large-diameter solid forgings by continuous casting, the compaction effect of the core of the billet is poor, so that the ultrasonic flaw detection defects of the finally obtained large-diameter solid forgings exceed the standard seriously.
[0004] In order to solve the above problems, the present invention provides a forging method for producing a large-diameter solid forging from a continuous casting billet, comprising:
[0005] Step S1, using two upper and lower cylindrical V-shaped anvils arranged opposite to each other to press the jaws of the columnar continuous casting billet to form a jaw section in the axial middle area of the columnar continuous casting billet to obtain a first intermediate billet; wherein, during the jaw pressing process, the single-pass pressing rate is 20-35%;
[0006] Step S2, dividing the first intermediate blank in half along the axial direction at the jaw section to obtain two second intermediate blanks; the second intermediate blank comprises a cylindrical forging blank body and a cylindrical clamp handle connected in sequence;
[0007] Step S3, using an upsetting assembly to upset the second intermediate blank to obtain a third intermediate blank;
[0008] Step S4, drawing the third intermediate billet to obtain a large-diameter solid forging.
[0009] Optionally, in step S3, the upsetting assembly includes an upsetting cover plate and an upsetting drain plate; the upsetting cover plate includes a cover plate body, a first through hole is provided at the axial center position of the cover plate body, the first through hole includes a first columnar groove and a first groove in a closed shape located at the upper end of the first columnar groove; the upsetting drain plate includes a drain plate body, a second through hole is provided at the axial center position of the drain plate body, the second through hole includes a second columnar groove and a second groove in a closed shape located at the upper end of the second columnar groove; the diameter of the forging blank body is D1, the diameter of the clamp handle is D2, the diameter of the first columnar groove is D3, the narrowest diameter of the second through hole is D4, the difference between D3 and D1 is 40-60 mm, and the difference between D4 and D2 is 40-60 mm;
[0010] In the step S3, the method of using an upsetting assembly to upset the second intermediate blank to obtain a third intermediate blank comprises:
[0011] Step S31, installing the second intermediate blank in the upsetting drain plate, so that the clamp handle is located in the second through hole and the lower end of the forging blank body is against the upper end surface of the upsetting drain plate;
[0012] Step S32, covering the upper end of the forging blank body with the cover plate body, so that the upper end of the forging blank body is located in the first columnar groove;
[0013] Step S33, applying pressure to the upper end of the second intermediate blank for upsetting, to obtain the third intermediate blank.
[0014] Optionally, the first through hole also includes a flared groove located at the upper end of the first groove, and an arc chamfer is provided between the inner wall of the first groove and the inner wall of the first columnar groove; the second through hole also includes a third columnar groove located at the upper end of the second groove, and an arc chamfer is provided on the upper inner wall of the third columnar groove.
[0015] Optionally, the opening angle of the V-shaped groove of the cylindrical V-shaped anvil is 110 degrees; the width of the cylindrical V-shaped anvil is 600 mm.
[0016] Optionally, the diameter D1 of the forging blank body is 1600 mm, the diameter D2 of the clamp handle is 1100 mm; the diameter D3 of the first columnar groove is 1650 mm, and the narrowest diameter of the second through hole is D4 is 1150 mm.
[0017] Optionally, the diameter D5 of the second columnar groove is 1400 mm.
[0018] Optionally, in step S2, the first intermediate blank is divided into two halves along its axial direction using a chopping knife.
[0019] Optionally, in step S1, the temperature of the columnar continuous casting billet is 1240-1260°C; in step S2, the temperature of the first intermediate billet is 1240-1260°C; in step S3, the temperature of the second intermediate billet is 1240-1260°C; in step S4, the temperature of the third intermediate billet is 1240-1260°C.
[0020] Optionally, the material of the columnar continuous casting billet includes one of 70Cr3Mo steel, 45Cr4NiMoV steel, YB-70 steel, YB-75 steel, 42CrMo steel, 30Cr1Mo1V steel, 30Cr2Ni4MoV steel and 25Cr2Ni4MoV steel.
[0021] The present invention also provides a solid forging, which is produced by the forging method for producing a large-diameter solid forging from a continuous casting billet as described above.
[0022] Compared with the prior art, the present invention uses upper and lower cylindrical V-shaped anvils to press the jaws on the axial middle area of the continuous casting billet to form a jaw section in the axial middle area of the columnar continuous casting billet, and then the continuous casting billet is divided at the jaw section for subsequent forging; in addition, after the material is divided, the jaw section is divided into two jaw handles, which is convenient for subsequent machine clamping and can also be used as a part of the forging product. Compared with the traditional use of upper flat and lower V-shaped anvils to press the jaws, the present invention uses upper and lower cylindrical V-shaped anvils to press the jaws, which can effectively limit the lateral widening of the billet, so that the core of the billet in the pressing jaw area is in a good three-dimensional compressive stress state, and a larger hydrostatic pressure and strain distribution can be obtained, so that the compaction effect of the billet in the jaw section is better, which is conducive to preventing gas from entering the billet after the billet is divided by the jaw section, thereby ensuring that the core of the billet has a better compaction effect during the subsequent forging process. In addition, in the present invention, by controlling the reduction rate during the jaw pressing process to be relatively high (20-35%), the holes in the core of the billet in the jaw section can be ensured to be closed, which is beneficial to prevent gas from entering the billet after the billet is divided by the jaw section, thereby further ensuring that the core of the billet has a better compaction effect during the subsequent forging process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic flow chart of a forging method for producing a large-diameter solid forging from a continuous casting billet in an embodiment of the present invention;
[0024] Figure 2 It is a schematic diagram of using two upper and lower cylindrical V-shaped anvils arranged opposite to each other to press the jaws of a columnar continuous casting billet in an embodiment of the present invention;
[0025] Figure 3 for Figure 2 AA section view of the middle cylindrical V-shaped anvil;
[0026] Figure 4 Schematic diagram of the structure of the first intermediate blank in an embodiment of the present invention;
[0027] Figure 5 It is a schematic diagram of using a chopping knife to divide the first intermediate blank into two halves along its axial direction at the jaw section in an embodiment of the present invention;
[0028] Figure 6 Schematic diagram of the structure of the second intermediate blank in an embodiment of the present invention;
[0029] Figure 7 This is one of the schematic diagrams of the second intermediate blank before being upset by the upsetting assembly in an embodiment of the present invention;
[0030] Figure 8 It is a schematic diagram of upsetting the second intermediate blank using the upsetting assembly in an embodiment of the present invention;
[0031] Fig. 9 Schematic diagram of the structure of the upsetting cover plate in an embodiment of the present invention;
[0032] Fig.10 It is a structural schematic diagram of an upsetting drain plate in an embodiment of the present invention;
[0033] Fig.11 The second schematic diagram is a diagram of the second intermediate blank before being upset by the upsetting assembly in the embodiment of the present invention;
[0034] Fig.12 Schematic diagram of the structure of a large diameter solid forging in an embodiment of the present invention.
[0035] Description of reference numerals:
[0036] 1. Cylindrical V-shaped anvil; 2. Columnar continuous casting billet; 3. First intermediate billet; 31. Jaw section; 4. Second intermediate billet; 41. Forging billet body; 42. Jaw handle; 5. Cover plate body; 51. First columnar groove, 52. First groove; 53. Expanding groove; 6. Leakage plate body; 61. Second columnar groove; 62. Second groove; 63. Second columnar groove; 7. Chopping knife; 8. Hammer; 9. Gasket. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0038] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0039] The term "including" and its variations used herein are open inclusions, i.e., "including but not limited to"; the term "based on" means "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more. It should be noted that the groove of the closed shape refers to the trend that the diameter of the groove gradually decreases from bottom to top; the flared groove refers to the trend that the diameter of the groove gradually increases from bottom to top.
[0040] like Figure 1 As shown, the present invention provided by the embodiment of the present invention provides a forging method for producing a large-diameter solid forging from a continuous casting billet, comprising:
[0041] Step S1: Figure 2 As shown, two upper and lower cylindrical V-shaped anvils 1 are used to press the jaws of the columnar continuous casting billet 2 to form a jaw section 31 in the axial middle area of the columnar continuous casting billet 2 to obtain a first intermediate billet 3, as shown in FIG. Figure 4 As shown; wherein, during the jaw pressing process, the single pass pressing rate is 20-35%;
[0042] Step S2: Figure 5 As shown, the first intermediate blank 3 is divided equally along its axial direction at the jaw section 31 to obtain two second intermediate blanks 4; Figure 6 As shown, the second intermediate blank 4 comprises a cylindrical forging blank body 41 and a cylindrical clamp handle 42 which are connected in sequence;
[0043] Step S3: Figure 7 and Figure 8 As shown, the second intermediate blank 4 is upset using an upsetting assembly to obtain a third intermediate blank;
[0044] Step S4, drawing the third intermediate billet to obtain a large-diameter solid forging; wherein the drawing process includes WHF drawing treatment and regular drawing. During the WHF drawing treatment, the flip angle is 90°, the reduction rates of the first four passes are 30%, 30%, 20% and 20% respectively, and the feed amount is full anvil.
[0045] The embodiment of the present invention uses upper and lower cylindrical V-shaped anvils 1 to press the jaws on the axial middle area of the continuous casting billet, so as to form a jaw section 31 in the axial middle area of the columnar continuous casting billet 2, and then the continuous casting billet is divided at the jaw section 31 for subsequent forging; in addition, after the division, the jaw section 31 is divided into two jaw handles 42, which is convenient for the subsequent operation machine to clamp, and can also be used as a part of the forging product. Compared with the traditional use of upper flat and lower V-shaped anvils to press the jaws, the embodiment of the present invention uses upper and lower cylindrical V-shaped anvils 1 to press the jaws, which can effectively limit the lateral widening of the billet, so that the core of the billet in the pressing jaw area is in a good three-dimensional compressive stress state, and a larger hydrostatic pressure and strain distribution can be obtained, so that the compaction effect of the billet in the jaw section 31 is better, which is conducive to preventing gas from entering the billet after the billet is divided by the jaw section 31, thereby ensuring that the core of the billet has a better compaction effect during the subsequent forging process. In addition, in the embodiment of the present invention, by controlling the reduction rate during the jaw pressing process to be relatively high (20-35%), it is possible to ensure that the holes in the core of the billet in the jaw section 31 are closed, which is beneficial in preventing gas from entering the billet after the billet is split by the jaw section 31, thereby further ensuring that the core of the billet has a better compaction effect during the subsequent forging process.
[0046] In some embodiments of the present invention, in step S3, Figure 7-10 As shown, the upsetting assembly includes an upsetting cover plate and an upsetting drain plate; Fig. 9 As shown, the upsetting cover plate includes a cover plate body 5, and a first through hole is provided at the axial center of the cover plate body 5. The first through hole includes a first columnar groove 51 and a first groove 52 in a closed shape located at the upper end of the first columnar groove 51; Fig.10 As shown, the upsetting leak plate includes a leak plate body 6, a second through hole is provided at the axial position of the leak plate body 6, and the second through hole includes a second columnar groove 61 and a second groove 62 in a closed shape located at the upper end of the second columnar groove 61; the diameter of the forging blank body 41 is D1, the diameter of the clamp handle 42 is D2, the diameter of the first columnar groove 51 is D3, the narrowest diameter of the second through hole is D4, the difference between D3 and D1 is 40-60 mm, and the difference between D4 and D2 is 40-60 mm;
[0047] like Figure 7-8 As shown, in the step S3, the upsetting assembly is used to upset the second intermediate blank 4 to obtain a third intermediate blank, including:
[0048] Step S31, installing the second intermediate blank 4 in the upsetting drain plate, so that the clamp handle 42 is located in the second through hole and the lower end of the forging blank body 41 is against the upper end surface of the upsetting drain plate;
[0049] Step S32, covering the upper end of the forging blank body 41 with the cover plate body 5, so that the upper end of the forging blank body 41 is located in the first columnar groove 51;
[0050] Step S33, applying pressure to the upper end of the second intermediate blank 4 for upsetting to obtain the third intermediate blank.
[0051] The traditional upsetting method is to upset the blank as a whole. The upsetting forging is relatively large, causing the radial shrinkage holes inside the blank to be pressed into an ellipsoidal shape. After being stretched, the radial shrinkage holes will extend in the axial direction, resulting in an increase in axial shrinkage holes, resulting in poor compaction effect of the blank. In this embodiment, the blank is upset by the upsetting cover plate and the upsetting drain plate, which can play a role in upsetting the part of the blank (corresponding to the large circular part of the forging), can reduce the upsetting forging ratio, and relatively increase the stretching ratio. In the compaction fire, the internal shrinkage holes and looseness can be effectively compacted, which is conducive to further improving the compaction effect of the blank. In addition, in this embodiment, the upper first groove 52 of the upsetting cover plate can also have an extrusion effect on the end of the blank, reducing the risk of cracking of the end of the blank during the subsequent stretching process.
[0052] In some embodiments of the present invention, in step S31, in order to ensure a reasonable blanking weight, a gasket 9 is provided at the top or bottom of the second intermediate blank 4 to increase the height. Figure 7 and Figure 8 As shown, a gasket 9 is provided at the top end of the second intermediate blank 4. Fig.11 As shown, a gasket 9 is provided at the bottom end of the second intermediate blank 4, and the lower end of the gasket 9 is supported by a movable platform. That is, the second intermediate blank 4 is installed in the upset drain pan, so that the clamp handle 42 is located in the second through hole and the lower end of the clamp handle 42 abuts against the gasket 9, so that the lower end of the forging blank body 41 abuts against the upper end surface of the upset drain pan. In this way, the weight of the blank inside the auxiliary tool (upsetting assembly) is reduced, excessive waste of materials is prevented, and production costs are reduced.
[0053] In some embodiments of the present invention, Fig. 9 and Fig.10 As shown, the first through hole also includes a flared groove 53 located at the upper end of the first groove 52, and an arc chamfer is provided between the inner wall of the first groove 52 and the inner wall of the first columnar groove 51; the second through hole also includes a third columnar groove 63 located at the upper end of the second groove 62, and the upper inner wall of the third columnar groove 63 is provided with an arc chamfer.
[0054] In some embodiments of the present invention, Figure 2 and Figure 3 As shown, the opening angle of the V-shaped groove of the cylindrical V-shaped anvil 1 is 110 degrees; the width L of the cylindrical V-shaped anvil 1 is 600 mm.
[0055] In some embodiments of the present invention, illustratively, Figure 6 As shown, the diameter D1 of the forging blank body 41 is 1600 mm, and the diameter D2 of the clamp handle 42 is 1100 mm; Fig. 9 and Fig.10 As shown, the diameter D3 of the first columnar groove 51 is 1650 mm, the narrowest diameter of the second through hole is D4 is 1150 mm, and the diameter D5 of the second columnar groove 61 is 1400 mm.
[0056] In some embodiments of the present invention, Figure 5 As shown, in step S2, the first intermediate blank 3 is bisected along its axial direction by a chopping knife 7. In this embodiment, the hammer, chopping knife 7, hydraulic press and operating machine are used to divide the material, so that the blank can be put into the furnace in time, thereby improving production efficiency.
[0057] In some embodiments of the present invention, in step S1, the temperature of the columnar continuous casting billet 2 is 1240-1260°C; in step S2, the temperature of the first intermediate billet 3 is 1240-1260°C; in step S3, the temperature of the second intermediate billet 4 is 1240-1260°C; in step S4, the temperature of the third intermediate billet is 1240-1260°C.
[0058] In some embodiments of the present invention, the material of the columnar continuous casting billet includes 70Cr3Mo steel, 45Cr4NiMoV steel, YB-70 steel, YB-75 steel, 42CrMo steel, 30Cr1Mo1V steel, 30Cr2Ni4MoV steel, 25Cr2Ni4MoV steel and other steel materials.
[0059] The embodiment of the present invention further provides a solid forging, which is produced by the forging method for producing a large-diameter solid forging from a continuous casting billet as described above.
[0060] The present invention will be further described below with reference to specific embodiments, taking the forging of a large diameter solid roll as an example.
[0061] Example 1
[0062] A1. Figure 2As shown, two upper and lower cylindrical V-shaped anvils 1 arranged opposite to each other are used to press the jaws of the columnar continuous casting billet 2 to form a jaw section 31 in the axial middle area of the columnar continuous casting billet 2 to obtain a first intermediate billet 3; wherein the material of the columnar continuous casting billet 2 is 70Cr3Mo steel; the opening angle of the V-shaped groove of the cylindrical V-shaped anvil 1 is 110 degrees, and the width L of the cylindrical V-shaped anvil 1 is 600mm; during the pressing jaw process, the single-pass reduction rate is 31.25%; the diameter D of the columnar continuous casting billet 2 is 1600mm, the length is 5900mm, and the temperature of the columnar continuous casting billet 2 is 1250℃.
[0063] A2. Figure 5 As shown, the first intermediate blank 3 is divided equally along its axial direction at the jaw section 31 to obtain two second intermediate blanks 4; wherein, as Figure 6 As shown, the second intermediate blank 4 includes a cylindrical forging blank body 41 and a cylindrical clamp handle 42 connected in sequence; the diameter D1 of the forging blank body 41 is 1600 mm, the diameter D2 of the clamp handle 42 is 1100 mm, and the temperature of the first intermediate blank 3 is 1250°C.
[0064] A3. Figure 7 As shown, the second intermediate blank 4 is installed in the upsetting drain plate, so that the clamp handle 42 is located in the second through hole and the lower end of the forging blank body 41 is against the upper end surface of the upsetting drain plate; the cover plate body 5 is covered on the upper end of the forging blank body 41, so that the upper end of the forging blank body 41 is located in the first columnar groove 51, and the gasket 9 is placed on the upper end surface of the forging blank body 41, as shown in FIG. Figure 8 As shown, the hammer 8 and the gasket 9 are used to apply pressure to the upper end of the second intermediate blank 4 to perform upsetting, thereby obtaining the third intermediate blank; wherein the temperature of the second intermediate blank 4 is 1250°C, as shown in FIG. Fig. 9 and Fig.10 As shown, the diameter D3 of the first columnar groove 51 is 1650 mm, and the narrowest diameter of the first through hole is D6 is 1150 mm; the diameter D5 of the second columnar groove 61 is 1400 mm, and the narrowest diameter of the second through hole is D4 is 1150 mm.
[0065] A4. The third intermediate billet is stretched to obtain a large diameter solid forging, wherein the stretching process includes a WHF stretching process and a regular stretching process. During the WHF stretching process, the turning angle is 90°, the reduction rates of the first four passes are 30%, 30%, 20% and 20% respectively, and the feed rate is full anvil. Fig.12 As shown; wherein, the temperature of the third intermediate blank is 1250°C, the large-diameter solid forging is a solid roll forging, and the diameter of the roll body is 1300mm.
[0066] Experimental example
[0067] The large diameter solid forgings prepared in Example 1 were subjected to heat treatment and then to flaw detection. The results were as follows: Fig.12 As shown, the hardness of part I of the forging is HSD40-45, the flaw detection result of the 1000mm diameter section of part I of the forging is Φ3.5, and the flaw detection result of the 860mm diameter section is Φ3; the hardness of part II of the forging is HSD65-69, and the flaw detection result of part II of the forging is Φ5; the hardness of part III of the forging is HSD40-45, and the flaw detection result of the 1000mm diameter section of part III of the forging is Φ3, and the flaw detection result of the 720mm diameter section is Φ2.5. It can be seen from the above results that the ultrasonic flaw detection results of the large-diameter solid forgings in the embodiment do not exceed the standard, indicating that the method of the present invention improves the compaction effect of the core of the billet.
[0068] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A forging method for producing large diameter solid forgings from continuous casting billets, characterized in that: include: Step S1, using two upper and lower cylindrical V-shaped anvils (1) arranged opposite to each other to press the jaws of the columnar continuous casting billet (2) to form a jaw section (31) in the axial middle area of the columnar continuous casting billet (2) to obtain a first intermediate billet (3); wherein, during the jaw pressing process, the single pass reduction rate is 20-35%; Step S2, bisecting the first intermediate blank (3) along its axial direction at the jaw section (31) to obtain two second intermediate blanks (4); the second intermediate blank (4) comprises a cylindrical forging blank body (41) and a cylindrical clamp handle (42) connected in sequence; Step S3, using an upsetting assembly to upset the second intermediate blank (4) to obtain a third intermediate blank; Step S4, drawing the third intermediate billet to obtain a large-diameter solid forging.
2. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: In the step S3, the upsetting assembly comprises an upsetting cover plate and an upsetting drain plate; the upsetting cover plate comprises a cover plate body (5), a first through hole is provided at the axial center position of the cover plate body (5), the first through hole comprises a first columnar groove (51) and a first groove (52) in a closed shape located at the upper end of the first columnar groove (51); the upsetting drain plate comprises a drain plate body (6), a second through hole is provided at the axial center position of the drain plate body (6), the second through hole comprises a second columnar groove (61) and a second groove (62) in a closed shape located at the upper end of the second columnar groove (61); the diameter of the forging blank body (41) is D1, the diameter of the clamp handle (42) is D2, the diameter of the first columnar groove (51) is D3, the narrowest diameter of the second through hole is D4, the difference between D3 and D1 is 40-60 mm, and the difference between D4 and D2 is 40-60 mm; In the step S3, the method of using an upsetting assembly to upset the second intermediate blank (4) to obtain a third intermediate blank comprises: Step S31, installing the second intermediate blank (4) in the upsetting drain plate, so that the clamp handle (42) is located in the second through hole and the lower end of the forging blank body (41) is against the upper end surface of the upsetting drain plate; Step S32, covering the upper end of the forging blank body (41) with the cover plate body (5), so that the upper end of the forging blank body (41) is located in the first columnar groove (51); Step S33, applying pressure to the upper end of the second intermediate blank (4) for upsetting to obtain the third intermediate blank.
3. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 2, characterized in that: The first through hole further comprises a flared groove (53) located at the upper end of the first groove (52), and an arc chamfer is provided between the inner wall of the first groove (52) and the inner wall of the first columnar groove (51); the second through hole further comprises a third columnar groove (63) located at the upper end of the second groove (62), and an arc chamfer is provided on the upper inner wall of the third columnar groove (63).
4. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: The opening angle of the V-shaped groove of the cylindrical V-shaped anvil (1) is 110 degrees; and the width of the cylindrical V-shaped anvil (1) is 600 mm.
5. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: The diameter D1 of the forging blank body (41) is 1600 mm, the diameter D2 of the clamp handle (42) is 1100 mm; the diameter D3 of the first columnar groove (51) is 1650 mm, and the narrowest diameter of the second through hole is D4 is 1150 mm.
6. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 5, characterized in that: The diameter D5 of the second columnar groove (61) is 1400 mm.
7. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: In the step S2, the first intermediate blank (3) is divided into two halves along its axial direction using a chopping knife (7).
8. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: In step S1, the temperature of the columnar continuous casting billet (2) is 1240-1260°C; in step S2, the temperature of the first intermediate billet (3) is 1240-1260°C; in step S3, the temperature of the second intermediate billet (4) is 1240-1260°C; in step S4, the temperature of the third intermediate billet is 1240-1260°C.
9. The forging method for producing large-diameter solid forgings from continuous casting billets according to claim 1, characterized in that: The material of the columnar continuous casting billet includes one of 70Cr3Mo steel, 45Cr4NiMoV steel, YB-70 steel, YB-75 steel, 42CrMo steel, 30Cr1Mo1V steel, 30Cr2Ni4MoV steel and 25Cr2Ni4MoV steel.
10. A solid forging, produced by the forging method for producing a large-diameter solid forging from a continuous casting billet as claimed in any one of claims 1 to 9.
Citation Information
Cited By
A forging process for producing a solid sun gear shaft from a continuous casting billet
CN123039274A