Casting method of special-shaped roller

By decomposing the blank of special-shaped roll into upper and lower sections and using a combination of sequential solidification and metallurgy, the problems of high waste rate and large material consumption in special-shaped roll casting are solved, the yield rate is improved, energy and materials are saved, and costs are reduced. .

CN119016687APending Publication Date: 2024-11-26SHANDONG PROVINCE SIFANG TECH DEV GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135951.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing special-shaped roll casting process has high waste rate and high material consumption, resulting in waste of energy and labor, and low yield and high cost.

Method used

The process of forming the two-casting molding is adopted to decompose the special-shaped roll blank into two symmetrical roll blanks with upper and lower sections, and cast by combining sequential solidification and metallurgy, and use lower cold iron and aluminum hot flux to improve casting efficiency and quality.

Benefits of technology

It significantly improves the yield rate of casting process, saves materials and energy, reduces production costs, and ensures the casting quality of special-shaped rolls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016687A_ABST
    Figure CN119016687A_ABST
Patent Text Reader

Abstract

According to the casting method for the special-shaped roller formed through two times of casting, an overall special-shaped roller blank is decomposed into an upper special-shaped roller blank and a lower special-shaped roller blank which are symmetrical in shape, the diameter of one end of each symmetrical special-shaped roller blank is small, the diameter of the other end of each symmetrical special-shaped roller blank is large, and during two times of casting, the end with the small diameter is located on the bottom face; and after the molten steel is cast, a sequence from bottom to top is naturally formed, so that the molten steel is cast in sequence from small diameter to large diameter. By means of two-time casting forming, the upper roller blank and the lower roller blank are metallurgically bonded into the whole special-shaped roller blank, the manufacturing problem of the curved-surface special-shaped roller with the two ends large in diameter and the middle small in diameter is solved, the yield of the casting technology for casting the special-shaped roller blank is increased by 25% or above, energy and materials are greatly saved, and the production cost is reduced. And the casting quality of the special-shaped roller is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a roll casting technology, in particular to a preparation method of a special-shaped roll by using two-time casting. Background Art

[0002] The rollers involved in the present invention include sizing rollers, tensioning rollers, straightening rollers for the production of seamless steel pipes, and most of the rollers in welded steel pipe units and cold-bent steel units. These rollers are all curved special-shaped rollers with large diameters at both ends and small diameters in the middle. When working, these rollers have to withstand strong rolling and sliding friction, repeated impacts on the head and tail of the rolled material, and the chilling and heating effects of high-temperature rolled materials and cooling water, resulting in a harsh working environment. Therefore, the above-mentioned special-shaped rollers are the most consumed workpieces in the production of seamless steel pipes, welded steel pipes and cold-bent steel.

[0003] Meanwhile, there are many varieties of special-shaped rollers, but the same specifications and varieties are in small batches. The weight of a finished roller can reach more than ten tons per piece, and the weight of a small roller is less than 5 kilograms per piece. At present, static casting is mostly used in casting of the special-shaped rollers. Since the middle section is small and easy to solidify first, the heat stagnation of the lower half cannot be solved, and defects such as looseness are easy to occur, resulting in waste. Increasing the riser to enhance the shrinkage compensation capacity is an effective way to solve the problem. The result is a low casting process yield, generally 40-50%, that is, consuming 1 ton of molten steel can only obtain 400-500 kilograms of roller blanks, resulting in great waste of energy, materials, labor, etc., and increasing the manufacturing and use costs. Summary of the invention

[0004] The present invention is to solve the problems of high scrap rate and high material consumption in the manufacture of existing curved profiled rollers, and proposes a process method for forming by two castings. The casting method of a profiled roller of the present invention is characterized in that the profiled roller blank is decomposed into two symmetrical upper and lower sections of the profiled roller blank, and the two sections are cast and formed, and the process method is as follows:

[0005] 1) The special-shaped roller blank is decomposed radially from the axial middle into two symmetrical and identically shaped roller blanks, one end of which has a small diameter and gradually increases in diameter toward the other end, and has the largest diameter at the other end surface; a central axis hole is provided in the middle of the special-shaped roller blank.

[0006] 2) The special-shaped roller blank is cast twice, and the casting mold design is that the end with a smaller diameter is at the bottom and the end with a larger diameter is at the top. After the molten steel is poured, it naturally solidifies in a sequence from bottom to top; a smaller riser is provided on the top of the special-shaped roller blank casting mold to meet the needs of shrinkage compensation;

[0007] 3) During the first casting, the casting of the lower section symmetrical roller blank is completed first; the first casting adopts the pouring channel, and the molten steel enters the cavity and gradually fills it from bottom to top. The temperature of the molten steel forms from low to high from bottom to top, and the cross-sectional area of ​​the casting mold increases from bottom to top, forming sequential solidification;

[0008] 4) taking out the cast lower section symmetrical roller blank, roughening and cleaning the surface of the end with the smaller diameter of the lower section symmetrical roller blank, and then setting the lower section symmetrical roller blank in the lower part of the cavity of the second casting mold, with the end with the smaller diameter upwardly exposed in the cavity, and setting a layer of thermite flux on the processed surface;

[0009] 5) Perform a second casting, i.e., perform casting of the upper symmetrical roller blank; ignite the thermite flux on the processing surface before casting to molten the processing surface, and promptly pour molten metal from the bottom runner after extinguishing the flame, and continuously pour in molten metal to continue heating the processing surface, so that the upper and lower symmetrical roller blanks are metallurgically bonded, thereby obtaining an integral special-shaped roller blank formed by two castings.

[0010] A further feature of the present invention is that, during the first casting, a lower chiller is installed at the lower part of the casting mold of the lower section symmetrical roller blank to enable the blank to be quickly and sequentially cooled and solidified; during the second casting, the lower section roller blank arranged at the lower part of the mold cavity plays the role of a lower chiller, further reducing the weight of the riser shrinkage compensation.

[0011] The present invention is also characterized in that the surface of the end with a smaller diameter of the lower section special-shaped roller blank is roughened and cleaned to completely remove the oxide scale and impurities on the surface. The roughening of the surface of the end with a smaller diameter of the lower section special-shaped roller blank is to process grooves on the end surface or make it uneven to obtain a larger surface area.

[0012] The thermite flux of the present invention is arranged on the surface of the end with the smaller diameter of the roughly processed lower section special-shaped roller blank. The thermite flux is ignited before casting and is completely fused with the cast metal melt to form a metallurgical bonding surface, thereby completing the preparation of the entire special-shaped roller blank.

[0013] The two castings of the special-shaped roller blank of the present invention are both made of the same metal material. When designing the blank, the required machining allowance is added to the surface of the end with the smaller diameter of the lower section special-shaped roller blank.

[0014] The special-shaped roller blank of the present invention has a small diameter at one end and gradually increases in diameter toward the other end to reach the maximum diameter at the other end face, or can have a maximum diameter when the end with a small diameter transitions to the other end face through an arc, and a central axis hole is provided in the middle of the special-shaped roller blank. The riser is a heat-insulating riser or a heat-generating heat-insulating riser.

[0015] The present invention is to overcome the problems of high scrap rate and high material consumption during the manufacturing of curved special-shaped rollers with large diameters at both ends and small diameters in the production of seamless steel pipes, welded steel pipes and cold-bent steel, and to provide a process method through two castings to solve the preparation problem of curved special-shaped rollers with large diameters at both ends and small diameters in the middle. The casting method of the present invention is simple and practical, and the casting process yield of the cast special-shaped roller blank is increased by more than 25%, which greatly saves energy and materials, reduces production costs, and ensures the casting quality of the special-shaped rollers. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a cross-sectional schematic diagram of the structure of the integral special-shaped roller blank of the present invention, wherein the diameters at both ends are large and gradually decrease toward the middle, with the middle diameter being the smallest. There is a central axis hole in the middle of the special-shaped roller blank.

[0017] Figure 2 It is a schematic diagram of the structural cross-section of a special-shaped roller blank decomposed into two upper and lower sections.

[0018] Figure 3 This is a schematic diagram of the casting sand mold cross section when the lower section symmetrical roller blank is cast for the first time:

[0019] Figure 4 This is a schematic diagram of the cross-section of the casting sand mold when the upper symmetrical roller blank is cast for the second time:

[0020] 1 is the lower section symmetrical roll blank obtained by the first casting, on the surface of the end with a smaller diameter, a groove is processed; 2 is the cavity of the upper section symmetrical roll blank cast by the second casting; 3 is the surface of the end with a smaller diameter of the lower section symmetrical roll blank, on which thermite flux is arranged; 4 is the runner, 5 is the riser, and 6 is the sand mold. DETAILED DESCRIPTION

[0021] The present invention will be described in detail below with reference to the accompanying drawings and exemplary embodiments. The following drawings show preferred embodiments, which do not limit other implementations of the present invention.

[0022] The present invention provides a two-time casting process for a curved special-shaped roller with large diameters at both ends and small diameter in the middle used in the production of seamless steel pipes, welded steel pipes and cold-bent steel. The method saves a lot of materials and can increase the casting process yield by more than 25%. The present invention is simple and practical to operate and ensures the casting quality of the special-shaped roller.

[0023] like Figure 1As shown, the present invention first improves the existing integral special-shaped roller blank, and decomposes the integral special-shaped roller blank into two symmetrical and identical roller blanks in the radial direction from the axial middle of the integral special-shaped roller blank, one end of which has a small diameter and gradually increases in diameter toward the other end, and has the largest diameter when it reaches the other end face, or the end with a small diameter has the largest diameter when it transitions to the other end face through an arc, and a central axis hole is provided in the middle of the special-shaped roller blank, such as Figure 2 shown.

[0024] The casting mold design of the special-shaped roller blank of the present invention makes the end with a smaller diameter at the bottom and the end with a larger diameter at the top during both castings. After the molten steel is cast, it naturally solidifies sequentially from bottom to top. A smaller riser 5 that can fully meet the shrinkage compensation requirements is arranged above the casting mold, or a heat-insulating riser or a heat-generating heat-insulating riser can also be used. During the first casting, a lower chill 7 is installed at the lower part of the lower section of the symmetrical roller blank casting mold to allow the blank to be rapidly cooled and solidified sequentially. During the second casting, the lower section of the roller blank at the lower part of the cavity plays the role of the lower chill 7, further reducing the weight of the riser 5 for shrinkage compensation.

[0025] Reference Figure 3 In the first casting, the present invention first completes the casting of the lower section symmetrical roller blank 1. The casting mold cavity 2 is designed with the end with a small diameter at the bottom and the end with a large diameter at the top, and a lower chiller 7 is provided. The first casting adopts the upper pouring channel casting. After the molten steel enters the cavity, it gradually fills up from bottom to top. The temperature of the molten steel forms from low to high from bottom to top. The cross-sectional area of ​​the casting mold increases from bottom to top, forming sequential solidification. In addition to the effect of the lower chiller 7, the present invention can fully meet the shrinkage compensation requirements of the casting blank by using a smaller riser, thereby ensuring the casting quality.

[0026] Next, the cast lower section symmetrical roller blank 1 is taken out, and then the surface of the end with a smaller diameter of the lower section symmetrical roller blank 1 is roughened and cleaned to remove the oxide scale and other debris on the end surface, and grooves are processed on the end surface with a smaller diameter or the end surface is made uneven to obtain a larger surface area.

[0027] Reference Figure 4 The processed and cleaned lower section symmetrical roll blank 1 is placed in the lower part of the second casting cavity 2, with the end with a small diameter upwardly exposed in the cavity 2, and a layer of thermite flux 3 is placed on its processed surface. Thermite flux 3 can utilize the superheated molten metal generated by the exothermic reaction between the metal oxide and the metal aluminum to heat the metal, thereby realizing the metallurgical bonding of the two sections of the symmetrical roll blank.

[0028] The second casting is performed, i.e., the casting of the upper symmetrical roller blank; the thermite flux 3 on the processing surface is ignited before casting, so that the processing surface is molten in a short time, and the molten metal is promptly cast from the runner 4 after the flame is extinguished. The continuously poured molten metal and thermite flux 3 continue to heat the processing surface, and the cross-sectional area of ​​the blank gradually increases from bottom to top. Under the action of the lower chill of the lower roller blank, a solidification sequence from bottom to top is formed, so that the upper and lower symmetrical roller blanks are metallurgically bonded in a molten state. The smoke and impurities generated by the combustion of thermite flux 3 are discharged from the riser 5, so as to obtain an integral special-shaped roller blank formed by two castings.

[0029] Since the shapes of the roller blanks cast twice can be naturally formed and solidified in sequence, and both times have the effect of lower chiller, the smaller riser provided in the present invention fully meets the shrinkage compensation demand of molten steel and achieves the purpose of improving the output rate of the casting process.

[0030] The two castings of the present invention all adopt the same metal material. When designing the blank, the required processing allowance is also designed on the surface of the end with a smaller diameter of the lower section symmetrical roller blank 1 to meet the needs of surface roughness processing.

[0031] Example 1

[0032] This embodiment is for manufacturing Φ159 seamless steel pipe unit sizing rollers. The original integral blank is cast by static casting, and the blank weight is 62kg and the pouring system weight is 76kg, totaling 138kg, that is, the required molten steel is 138kg, the casting process yield is 45%, and high chromium cast iron material is used for casting.

[0033] Refer to the attached Figures 1 to 4 The design dimensions of the special-shaped roller blank after decomposition in this embodiment are: the large diameter end is Φ312mm, the small diameter end is Φ236mm, the inner hole is Φ120mm, the height design of the upper section special-shaped roller blank is 91mm, and the lower section special-shaped roller blank is 94mm, and the axial processing amount of the small diameter end face is increased by 3mm.

[0034] The two casting mold cavities 2 of the present embodiment are designed with the end with a smaller diameter at the bottom and the end with a larger diameter at the top. With the effect of the lower chiller 7 or the lower section roller blank 1, the molten steel naturally solidifies in sequence from bottom to top after being cast. Therefore, a smaller riser 5 can be designed to meet the needs of shrinkage compensation.

[0035] First, the casting of the lower symmetrical roller blank 1 is completed, and the casting mold is set as follows Figure 3As shown. The first casting is cast using the upper pouring channel 4. After the molten steel enters the cavity 2, it gradually fills up from bottom to top. The temperature of the molten steel forms from low to high from bottom to top. The cross-sectional area of ​​the mold increases from bottom to top, forming sequential solidification. Through the cooling effect of the lower chiller 7, a smaller insulation riser 5 is used. The first casting of the lower section symmetrical roller blank 1 actually uses 44kg of molten steel to obtain a 32kg blank.

[0036] The lower symmetrical roller blank 1 which has been cast is taken out, and the surface of the end with a smaller diameter of the blank is roughened and cleaned, and then the processed and cleaned lower symmetrical roller blank 1 is set in the lower part of the mold cavity 2 of the second casting mold, and the end with a smaller diameter is exposed upward in the mold cavity 2, and a layer of thermite flux 3 is set thereon;

[0037] Then the second casting is carried out to cast the upper symmetrical roller blank; before casting, the thermite flux 3 on the processing surface is ignited to produce a molten state, and after the flame is extinguished, the molten metal is cast from the bottom runner 4 in time to continue heating the processing surface. The continuously poured molten metal and the molten state produced by the thermite flux 3, under the joint action of the two, produce metallurgical bonding between the upper and lower symmetrical roller blanks, so that the two symmetrical roller blanks are fused into an integral special-shaped roller blank. Due to the lower cold iron effect produced by the lower roller blank 1, the cross-sectional area of ​​the roller blank gradually increases from bottom to top to form a sequential solidification from bottom to top. The design of the bottom runner 4 allows the smoke and a small amount of impurities generated by the combustion of thermite flux 3 to be discharged from the heating and heat preservation riser 5. The second casting of the upper symmetrical roller blank actually uses 45kg of molten steel, and the two castings actually use a total of 89kg of molten steel. The overall blank weighs 62.5kg, and the process yield rate is 70.2%, which is 25.2% higher than the overall static casting method, saving 49kg of molten steel.

[0038] The integral special-shaped roller blank formed by two castings becomes a finished product through heat treatment and mechanical processing. After passing the ultrasonic flaw detection, it is put into trial use on the machine. After multiple processing and repair, no quality problems are found, which fully meets the actual use needs.

[0039] Example 2

[0040] This embodiment is to manufacture the precision forming roll of the ERW welded steel pipe unit. The original integral blank is cast by static casting, and the blank weight is 65kg (1 piece) and the pouring and rigging system weight is 76kg, totaling 141kg, that is, the required molten steel is 141kg, and the casting process yield is 46%. Blank size: maximum diameter is Φ275mm, minimum diameter is Φ209mm, inner hole is Φ100mm, roller height is 232mm, and high chromium cast iron material is used for casting.

[0041] Refer to the attached Figures 1 to 4The dimensions of the decomposed special-shaped roller blank in this embodiment are: the large diameter end is Φ275mm, the small diameter end is Φ209mm, the inner hole is Φ100mm, the height of the upper section special-shaped roller blank is designed to be 116mm, and the height of the lower section special-shaped roller blank is 119mm, and the axial processing amount of the small diameter end face is increased by 3mm.

[0042] The double casting mold cavity 2 of this embodiment also has a small diameter end at the bottom and a large diameter end at the top. With the cooling effect of the lower chiller 7 or the lower section roller blank 1, the molten steel is naturally solidified from bottom to top after being cast, and a smaller heating and heat preservation riser 5 is used.

[0043] The mold settings are as follows Figure 3 As shown, the first casting adopts the upper pouring channel 4. After the molten steel enters the cavity 2, it gradually fills up from bottom to top. The temperature of the molten steel forms from low to high from bottom to top. The cross-sectional area of ​​the mold increases from bottom to top. In addition, the effect of the lower chiller 7 forms a sequential solidification. The first casting of the lower section symmetrical roller blank 1 actually uses 45.5 kg of molten steel to obtain a 33 kg blank. The cast lower section symmetrical roller blank 1 is taken out, and the surface of the end with a small diameter is roughened and cleaned. After that, it is set in the lower part of the cavity 2 of the second casting mold, and a layer of aluminum thermal flux 3 is set on the end exposed to the small diameter of the cavity 2.

[0044] The second casting of the upper symmetrical roller blank is carried out; before casting, the thermite flux 3 is ignited to make the processed surface molten, and after the flame is extinguished, the molten metal is cast from the runner 4 as soon as possible to make the upper and lower symmetrical roller blanks metallurgically bonded, thereby completing the casting of the overall special-shaped roller blank. The roller blank is solidified sequentially from bottom to top to ensure the casting quality. The smoke and impurities generated during casting are discharged from the heating and insulation riser 5. The second casting of the upper symmetrical roller blank actually uses 46kg of molten steel, and the two castings actually use a total of 91.5kg of molten steel. The overall blank weighs 65.3kg, and the process yield is 71.4%, which is 25.4% higher than the overall static casting method, saving 49.5kg of molten steel.

[0045] The special-shaped roller blank formed by twice casting in this embodiment has no casting quality problems after multiple processing and repair, which provides another production method for the preparation of special-shaped roller blanks.

[0046] The curved surface special-shaped roller blank produced by the present invention saves a large amount of molten steel, saves a large amount of metal smelting energy consumption and metal smelting burning loss, and produces good economic and social benefits.

[0047] The present invention is not limited to the above embodiments, and various deformations and modifications can be made without departing from the design concept of the present invention. These changes and modifications all belong to the protection scope of the present invention.

Claims

1. A method for casting a special-shaped roll, characterized in that: The special-shaped roller blank is decomposed into two symmetrical sections, and then cast twice. The process is as follows: 1) Decomposing the special-shaped roller blank from the axial middle along the radial direction into two symmetrical and identically shaped roller blanks, one end of which has a small diameter and gradually increases in diameter toward the other end, and has the largest diameter at the other end surface; the center of the special-shaped roller blank has a central axis hole; 2) The special-shaped roller blank is cast twice, and the casting mold design is that the end with a smaller diameter is at the bottom and the end with a larger diameter is at the top. After the molten steel is poured, it naturally solidifies in a sequence from bottom to top; a smaller riser is provided on the top of the special-shaped roller blank casting mold to meet the needs of shrinkage compensation; 3) During the first casting, the casting of the lower section symmetrical roller blank is completed first; the first casting adopts the pouring channel, and the molten steel enters the cavity and gradually fills it from bottom to top. The temperature of the molten steel forms from low to high from bottom to top, and the cross-sectional area of ​​the casting mold increases from bottom to top, forming sequential solidification; 4) taking out the cast lower section symmetrical roller blank, roughening and cleaning the surface of the end with the smaller diameter of the lower section symmetrical roller blank, and then setting the lower section symmetrical roller blank in the lower part of the cavity of the second casting mold, with the end with the smaller diameter upwardly exposed in the cavity, and setting a layer of thermite flux on the processed surface; 5) Perform a second casting, i.e., perform casting of the upper symmetrical roller blank; ignite the thermite flux on the processing surface before casting to molten the processing surface, and promptly pour molten metal from the bottom runner after extinguishing the flame, and continuously pour in molten metal to continue heating the processing surface, so that the upper and lower symmetrical roller blanks are metallurgically bonded, thereby obtaining an integral special-shaped roller blank formed by two castings.

2. The casting method according to claim 1, characterized in that: During the first casting, a lower chiller is installed at the lower part of the lower section symmetrical roller blank casting mold to enable the blank to be cooled and solidified quickly and sequentially.

3. The casting method according to claim 1, characterized in that: During the second casting, the lower roller blank arranged at the lower part of the cavity plays the role of lower chiller, further reducing the weight of the riser shrinkage compensation.

4. The casting method according to claim 1, characterized in that: The surface of the end with the smaller diameter of the lower section special-shaped roller blank is roughened and cleaned to completely remove the oxide scale and sundries on the surface.

5. The casting method according to claim 4, characterized in that: The roughening process is performed on the end surface with a small diameter of the lower section special-shaped roller blank, that is, grooves are processed on the end surface or the end surface is made uneven to obtain a larger surface area.

6. The casting method according to claim 1 or 5, characterized in that: The thermite flux is arranged on the surface of the end with the smaller diameter of the roughly processed lower section special-shaped roller blank. The thermite flux is ignited before casting and is completely fused with the cast metal melt to form a metallurgical bonding surface, thereby completing the preparation of the entire special-shaped roller blank.

7. The casting method according to claim 1, characterized in that: The same metal material is used for the two castings of the special-shaped roller blank.

8. The casting method according to claim 4 or 5, characterized in that: When designing the blank, the required machining allowance is added to the surface of the end with the smaller diameter of the lower section special-shaped roller blank.

9. The casting method according to claim 1, characterized in that: The end of the special-shaped roller blank with a smaller diameter can also transition to the other end face through an arc so that the diameter is the largest. The middle of the special-shaped roller blank has a central axis hole.

10. The casting method according to claim 1, characterized in that: The riser is a heat-insulating riser or a heat-generating heat-insulating riser.