Welding wire for welding TP347H-12Cr1MoV dissimilar materials and preparation method thereof

By preparing TP347H-12Cr1MoV welding wire for dissimilar material welding, the problems of poor joint quality and high residual stress of dissimilar steels were solved, achieving high-temperature service performance and metallurgical bonding, and making it suitable for MAG/MIG and TIG welding.

CN119016934APending Publication Date: 2024-11-26XIAN THERMAL POWER RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160633.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Dissimilar steel joints exhibit differences in chemical composition, microstructure, and mechanical properties during the welding process, leading to poor joint quality, high residual stress, and premature failure during service.

Method used

The TP347H-12Cr1MoV dissimilar material welding wire is used. The core is composed of Fe powder, Mo powder, Nb+Ta powder, Mn powder, Si powder, Ti powder, Re powder and Ni powder. The welding skin is Cr30Ni70 strip. It is prepared by vacuum heating, mixing and drawing to form a nickel-based welding wire to achieve metallurgical bonding and excellent high-temperature performance.

Benefits of technology

It effectively reduces the differences in thermophysical properties between dissimilar steels, improves welding quality, reduces residual stress, and ensures high-temperature service performance. It is suitable for MAG/MIG and TIG welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016934A_ABST
    Figure CN119016934A_ABST
Patent Text Reader

Abstract

The invention provides a welding wire for welding TP347H-12Cr1MoV dissimilar materials and a preparation method of the welding wire, and belongs to the technical field of metal materials. The welding wire comprises a flux core and a welding skin, the flux core comprises, by mass, 40%-50% of Fe powder, 10%-15% of Mo powder, 5%-10% of Nb + Ta powder, 5%-10% of Mn powder, 1%-2% of Si powder, 1%-2% of Ti powder, 1%-3% of Re powder and the balance Ni powder, and the sum of the mass percent of the components is 100%. The welding wire has fewer alloy elements, takes Ni as a matrix, is good in toughness, and has a linear expansion coefficient between the two kinds of steel, so that the problem of large welding residual stress concentration caused by thermophysical property difference between dissimilar steel can be effectively solved, meanwhile, excellent connection between the welding wire and the steel on the two sides can be ensured, and the welding wire has good high-temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to a TP347H-12Cr1MoV welding wire for welding dissimilar materials and a preparation method thereof. Background Art

[0002] In order to continuously improve the power generation efficiency of thermal power units, thermal power units are gradually developing towards high parameters and large capacity, and the steam temperature and pressure of the units will inevitably increase. In order to ensure the safe operation of the units and take into account economic cost factors, many units use austenitic heat-resistant steels, such as TP347H, Super304H, HR3C, etc., at the outlet of the high-temperature section of the heating surface pipe system of the boiler, and ferritic steels, such as T91, T22, 12Cr1MoV, etc., are mostly used on the inlet side. This inevitably leads to a large number of dissimilar steel welding joints of austenitic steel and ferritic steel, such as TP347H / T91, TP347H / 12Cr1MoV, TP347H / T22, HR3C / T91, etc.

[0003] However, dissimilar steel joints have always been the weak point of boiler heating surface tubes. This is mainly due to the differences in chemical composition, microstructure and mechanical properties of dissimilar steels, which result in "innate" deficiencies in the joints, such as dilution of alloy elements in the weld, decarburization layer produced by carbon migration, mismatched creep strength, large difference in expansion coefficient, easy oxidation notch on the low alloy steel side, and residual stress in the joints. Although the above adverse effects can be weakened to a certain extent by optimizing the welding process, its essence cannot be changed. There are still problems such as poor quality of dissimilar steel connections, large residual stress in dissimilar steel joints, and premature failure during service.

[0004] Therefore, selecting matching welding materials is the most fundamental solution to ensure the safety and reliability of dissimilar steel joints. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides a TP347H-12Cr1MoV welding wire for welding dissimilar materials and a preparation method thereof.

[0006] In one aspect of the present invention, a TP347H-12Cr1MoV welding wire for welding dissimilar materials is provided, the welding wire comprising: a flux core and a welding skin; wherein the flux core comprises:

[0007] 40-50% Fe powder;

[0008] 10~15% powder;

[0009] 5-10% Nb+Ta powder;

[0010] 5-10% Mn powder;

[0011] 1-2% Si powder;

[0012] 1-2% Ti powder;

[0013] 1-3% Re powder;

[0014] The rest is Ni powder, and the sum of the mass percentages of the above components is 100%.

[0015] Optionally, the powder particle size in the drug core is 100-200 meshes.

[0016] Optionally, the filling rate of the drug core is 20-22%.

[0017] Optionally, the welding skin is Cr30Ni70 strip.

[0018] Optionally, the Cr30Ni70 strip has a thickness of 0.1-0.5 mm and a width of 5-10 mm.

[0019] Another aspect of the present invention provides a method for preparing the TP347H-12Cr1MoV welding wire for welding dissimilar materials as described above, the method comprising:

[0020] Weigh the powders according to mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder, and the sum of the mass percentages of the above components is 100%;

[0021] The weighed drug powders are placed in a vacuum heating furnace for heating, and after drying, are placed in a powder mixer for mixing to obtain drug core powder;

[0022] A Cr30Ni70 strip is used as a welding skin, and the flux core powder is wrapped in the Cr30Ni70 strip by a flux cored wire drawing device, and the welding wire is obtained by a drawing process.

[0023] Optionally, the heating treatment is performed at a temperature of 250-300° C. and for a time of 1-4 h.

[0024] Optionally, the aperture of the first drawing die in the drawing process is 2.6 mm, and during the drawing process, the aperture of the die decreases successively.

[0025] Optionally, the diameter of the welding wire is 1-1.5 mm.

[0026] The present invention provides a TP347H-12Cr1MoV welding wire for dissimilar material welding and a preparation method thereof, wherein the welding wire comprises: a flux core and a welding skin, the flux core comprises: 40-50% Fe powder, 10-15% Mo powder, 5-10% Nb+Ta powder, 5-10% Mn powder, 1-2% Si powder, 1-2% Ti powder, 1-3% Re powder, and the rest is Ni powder, and the sum of the mass percentages of the above components is 100%. The welding wire has fewer alloy elements, takes Ni as a matrix, has good toughness, and a linear expansion coefficient that is between the above two steels, thereby effectively reducing the problem of large welding residual stress concentration caused by the difference in thermophysical properties between dissimilar steels, and at the same time can ensure its excellent connection with the steels on both sides, and has good high temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A flowchart of a method for preparing a TP347H-12Cr1MoV welding wire for welding dissimilar materials according to an embodiment of the present invention;

[0028] Figure 2 The metallographic structure of the weld obtained by welding TP347H / 12Cr1MoV dissimilar steel using the nickel-based welding wire prepared in Example 2 of the present invention;

[0029] Figure 3 The metallographic structure of the weld obtained by welding TP347H / 12Cr1MoV dissimilar steels using the nickel-based welding wire prepared in Example 2 of the present invention and the interface of 12Cr1MoV;

[0030] Figure 4 The metallographic structure of the weld obtained by welding TP347H / 12Cr1MoV dissimilar steels using the nickel-based welding wire prepared in Example 2 of the present invention and the interface of TP347H;

[0031] Figure 5 The tensile fracture morphology of the joint obtained by welding TP347H / 12Cr1MoV dissimilar steels using the nickel-based welding wire prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present invention and are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0033] In one aspect of the present invention, a TP347H-12Cr1MoV welding wire for welding dissimilar materials is provided, the welding wire comprising: a flux core and a weld skin; wherein the flux core is filled in the weld skin, wherein the flux core is composed of the following components by mass percentage: 40-50% Fe powder, 10-15% Mo powder, 5-10% Nb+Ta powder, 5-10% Mn powder, 1-2% Si powder, 1-2% Ti powder, 1-3% Re powder, and the rest is Ni powder, and the sum of the mass percentages of the above components is 100%.

[0034] It should be understood that the welding wire of this embodiment acts on TP347H and 12Cr1MoV, both of which have Fe as their main alloying element. From the Fe-Ni binary phase diagram, it can be seen that Ni and Fe can be infinitely solid-dissolved. Therefore, the main element in the welding wire of this embodiment is Ni, so that the nickel-based welding wire can achieve metallurgical bonding of TP347H and 12Cr1MoV dissimilar steels. In addition, TP347H austenitic stainless steel contains a certain amount of Ni element, so the nickel-based welding wire of this embodiment can achieve high-quality connection with TP347H.

[0035] Furthermore, since TP347H / 12Cr1MoV needs to serve in the boiler at high temperature for a long time, the TP347H / nickel-based weld / 12Cr1MoV heterogeneous joint formed by nickel-based welding wire will inevitably diffuse elements at high temperature. Therefore, in this embodiment, a certain amount of Fe element is added to the welding wire powder: Fe and Ni can be infinitely dissolved, and the addition of Fe element to the nickel-based weld can improve the fluidity of the nickel-based molten pool, improve welding formation, and reduce welding defects on the one hand; on the other hand, the Fe element ensures the metallurgical bonding performance between the steel matrix on both sides, and reduces the component diffusion problem caused by the large difference in alloy elements. In other words, when there is a certain amount of Fe element in the nickel-based weld, the difference in chemical composition between the nickel-based weld and the steel matrix on both sides is greatly reduced, thereby alleviating the failure problem of the 12Cr1MoV low-alloy element side steel in the TP347H / 12Cr1MoV heterogeneous joint during long-term service at high temperature.

[0036] Furthermore, a certain amount of Nb+Ta elements are added to the welding wire powder of this embodiment, wherein Nb and Ta can be dissolved in the Ni matrix, effectively improving the strength of the nickel-based weld, which is similar to the solid solution strengthening effect of Mo; Nb is a strong carbide-forming element, which can fix the C element at the interface of TP347H / nickel-based weld and nickel-based weld / 12Cr1MoV, thereby avoiding the carbon migration problem of TP347H / nickel-based weld / 12Cr1MoV dissimilar joints under high temperature and long-term service.

[0037] Furthermore, Mn and Si elements are added to the welding wire powder of this embodiment, which, on the one hand, play a role in deoxidation and reduce the porosity defects in the weld; on the other hand, Mn is an austenite-forming element, and the addition of Mn element can improve the bonding performance between the nickel-based weld and the TP347H side.

[0038] Furthermore, a certain amount of rare earth Re element is added to the welding wire powder of this embodiment. Since nickel-based welds are often single-phase austenite structures with coarse grains, they are prone to weak grain boundary bonding strength. Rare earth elements can purify grain boundaries and refine grains, thereby preventing the formation of creep holes at grain boundaries of nickel-based welds at high temperatures, thereby improving the high-temperature strength of nickel-based welds.

[0039] In some preferred embodiments, the particle size of the powder in the drug core is 100-200 meshes, and the purity of the powder is ≥99.90%.

[0040] In other preferred embodiments, the filling rate of the drug core is 20-22%.

[0041] Furthermore, generally speaking, TP347H / 12Cr1MoV dissimilar steels are used at high temperatures, wherein the maximum use temperature of TP347H steel can reach 700°C, and the normal use temperature of 12Cr1MoV steel in boilers is generally 480-580°C, so the designed nickel-based welds also need to be used at high temperatures. Therefore, the weld skin of this embodiment uses Cr30Ni70 strip, to which Cr element is added, and Cr element can form Cr2O3 dense oxide at high temperature to protect the nickel-based weld from high temperature oxidation; in addition, according to the Ni-Cr binary phase diagram, it can be seen that the solid solubility of Cr in Ni is very high, and the solid solution of Cr can improve the strength of Ni, thereby ensuring the high temperature strength of the dissimilar steel joint.

[0042] In other preferred embodiments, the welding skin is a Cr30Ni70 strip with a thickness of 0.1 to 0.5 mm and a width of 5 to 10 mm.

[0043] As a further preferred solution, the thickness of the Cr30Ni70 strip is 0.2 mm, 0.3 mm, 0.4 mm, and the width is 6 mm, 7 mm, 8 mm, 9 mm, etc.

[0044] The welding wire provided in this embodiment not only takes into account the connection quality of TP347H and 12Cr1MoV, but also focuses on the high-quality connection with 12Cr1MoV, thereby solving the problems of large residual stress in such dissimilar steel joints and premature failure during service.

[0045] like Figure 1As shown, another aspect of the present invention provides a method S100 for preparing the TP347H-12Cr1MoV welding wire for dissimilar materials welding as described above, which specifically includes the following steps S110 to S130:

[0046] S110. Weigh the powders according to mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%.

[0047] S120, placing the weighed drug powders in a vacuum heating furnace for heating treatment, and after drying, placing in a powder mixer for mixing to obtain drug core powder.

[0048] In some preferred embodiments, the temperature of the heating treatment is 250-300°C, for example, 250°C, 260°C, 270°C, 280°C, 290°C, etc., and the time is 1-4h, for example, 1h, 2h, 3h, 4h. The above heating treatment removes the crystal water in the powder.

[0049] In other preferred embodiments, the powder is mixed in the powder mixer for preferably 1-4 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, etc.

[0050] S130, using Cr30Ni70 strip as welding skin, the flux core powder is wrapped in the Cr30Ni70 strip through the flux cored wire drawing equipment, and the welding wire is obtained after drawing treatment.

[0051] It should be noted that before wrapping the flux core powder in the Cr30Ni70 belt, alcohol should be used to remove grease on the surface of the Cr30Ni70 belt, and then the flux powder should be wrapped in the Cr30Ni70 belt through the flux cored wire drawing equipment.

[0052] In some preferred embodiments, the first drawing die aperture of the drawing process is 2.6 mm, and during the drawing process, the die aperture decreases successively.

[0053] In other preferred embodiments, the diameter of the welding wire is 1-1.5 mm, such as 1 mm, 1.2 mm, 1.3 mm, 1.5 mm, etc.

[0054] It should also be understood that the welding wire obtained after the drawing process can also be wound on a welding wire reel by a wire winding machine, and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0055] The welding wire developed by the method of the present invention requires fewer types of powders, has a simple preparation process, and is convenient for large-scale batch production.

[0056] The welding wire prepared by the method of the present invention preferably has a wire diameter of 1.2 mm, can be used for MAG / MIG welding, and can also be used for TIG welding, and has wide adaptability. It has excellent mechanical properties, a tensile strength of 440-461 MPa, an elongation after fracture of 24-28%, and a room temperature impact toughness of 90-98 J.

[0057] The preparation method of TP347H-12Cr1MoV welding wire for welding dissimilar materials will be further described below in conjunction with specific examples:

[0058] Example 1

[0059] The preparation method of the TP347H-12Cr1MoV welding wire for welding dissimilar materials in this example includes the following steps:

[0060] Step 1: Weigh the powders by mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%;

[0061] Step 2: The powder weighed in step 1 is placed in a vacuum heating furnace and heated at a temperature of 250-300° C. for 1-4 hours to remove the crystal water in the powder; the dried powder is placed in a powder mixer for sufficient mixing, and the mixing time is 1-4 hours;

[0062] Step 3: Use Cr30Ni70 strip as welding skin, use alcohol to remove grease on the surface of Cr30Ni70 strip, and wrap the powder prepared in step 2 in the Cr30Ni70 strip through flux-cored wire drawing equipment. The aperture of the first drawing die is 2.6 mm;

[0063] Step 4: After the first drawing process is completed, the die aperture is reduced successively, and finally a flux-cored welding wire with a diameter of 1.2 mm is obtained;

[0064] Step 5: After the flux-cored welding wire is drawn, it is wound on the welding wire reel by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0065] The nickel-based flux-cored welding wire prepared in Example 1 was used for TP347H / 12Cr1MoV dissimilar steel butt welding. After testing, the mechanical properties of the dissimilar steel welded joints were as follows: tensile strength 450MPa, elongation after fracture 24%, and room temperature impact toughness 90J.

[0066] Example 2

[0067] The preparation method of the TP347H-12Cr1MoV welding wire for welding dissimilar materials in this example includes the following steps:

[0068] Step 1: Weigh the powders by mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%;

[0069] Step 2: The powder weighed in step 1 is placed in a vacuum heating furnace and heated at a temperature of 250-300° C. for 1-4 hours to remove the crystal water in the powder; the dried powder is placed in a powder mixer for sufficient mixing, and the mixing time is 1-4 hours;

[0070] Step 3: Use Cr30Ni70 strip as welding skin, use alcohol to remove grease on the surface of Cr30Ni70 strip, and wrap the powder prepared in step 2 in the Cr30Ni70 strip through flux-cored wire drawing equipment. The aperture of the first drawing die is 2.6 mm;

[0071] Step 4: After the first drawing process is completed, the die aperture is reduced successively, and finally a flux-cored welding wire with a diameter of 1.2 mm is obtained;

[0072] Step 5: After the flux-cored welding wire is drawn, it is wound on the welding wire reel by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0073] The nickel-based flux-cored welding wire prepared in Example 2 was used for TP347H / 12Cr1MoV dissimilar steel butt welding. After testing, the mechanical properties of the dissimilar steel welded joints were as follows: tensile strength 440 MPa, elongation after fracture 28%, and room temperature impact toughness 93 J.

[0074] Figure 2 This is the metallographic structure of the weld in this embodiment. It can be seen from the figure that the weld is mainly composed of columnar dendrites, the structure is uniform, and no defects are found.

[0075] Figure 3 This is the metallographic structure of the interface between the nickel-based weld and 12Cr1MoV. As can be seen from the figure, the interface is clear, the two materials are metallurgically bonded, and no defects are observed.

[0076] Figure 4 This is the metallographic structure of the interface between the nickel-based weld and TP347H. As can be seen from the figure, the interface is clear, the two materials are metallurgically bonded, and no defects are observed.

[0077] Figure 5 This is the tensile fracture morphology of the TP347H / 12Cr1MoV dissimilar steel joint. It can be seen from the figure that the fracture is mainly characterized by dimple morphology.

[0078] Example 3

[0079] The preparation method of the TP347H-12Cr1MoV welding wire for welding dissimilar materials in this example includes the following steps:

[0080] Step 1: Weigh the powders by mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%;

[0081] Step 2: The powder weighed in step 1 is placed in a vacuum heating furnace and heated at a temperature of 250-300° C. for 1-4 hours to remove the crystal water in the powder; the dried powder is placed in a powder mixer for sufficient mixing, and the mixing time is 1-4 hours;

[0082] Step 3: Use Cr30Ni70 strip as welding skin, use alcohol to remove grease on the surface of Cr30Ni70 strip, and wrap the powder prepared in step 2 in the Cr30Ni70 strip through flux-cored wire drawing equipment. The aperture of the first drawing die is 2.6 mm;

[0083] Step 4: After the first drawing process is completed, the die aperture is reduced successively, and finally a flux-cored welding wire with a diameter of 1.2 mm is obtained;

[0084] Step 5: After the flux-cored welding wire is drawn, it is wound on the welding wire reel by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0085] The nickel-based flux-cored welding wire prepared in Example 3 was used for TP347H / 12Cr1MoV dissimilar steel butt welding. After testing, the mechanical properties of the dissimilar steel welded joints were as follows: tensile strength 458MPa, elongation after fracture 25%, and room temperature impact toughness 97J.

[0086] Example 4

[0087] The preparation method of the TP347H-12Cr1MoV welding wire for welding dissimilar materials in this example includes the following steps:

[0088] Step 1: Weigh the powders by mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%;

[0089] Step 2: The powder weighed in step 1 is placed in a vacuum heating furnace and heated at a temperature of 250-300° C. for 1-4 hours to remove the crystal water in the powder; the dried powder is placed in a powder mixer for sufficient mixing, and the mixing time is 1-4 hours;

[0090] Step 3: Use Cr30Ni70 strip as welding skin, use alcohol to remove grease on the surface of Cr30Ni70 strip, and wrap the powder prepared in step 2 in the Cr30Ni70 strip through flux-cored wire drawing equipment. The aperture of the first drawing die is 2.6 mm;

[0091] Step 4: After the first drawing process is completed, the die aperture is reduced successively, and finally a flux-cored welding wire with a diameter of 1.2 mm is obtained;

[0092] Step 5: After the flux-cored welding wire is drawn, it is wound on the welding wire reel by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0093] The nickel-based flux-cored welding wire prepared in Example 4 was used for TP347H / 12Cr1MoV dissimilar steel butt welding. After testing, the mechanical properties of the dissimilar steel welded joints were as follows: tensile strength 461 MPa, elongation after fracture 26%, and room temperature impact toughness 98 J.

[0094] Example 5

[0095] The preparation method of the TP347H-12Cr1MoV welding wire for welding dissimilar materials in this example includes the following steps:

[0096] Step 1: Weigh the powders by mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder. The sum of the mass percentages of the above components is 100%;

[0097] Step 2: The powder weighed in step 1 is placed in a vacuum heating furnace and heated at a temperature of 250-300° C. for 1-4 hours to remove the crystal water in the powder; the dried powder is placed in a powder mixer for sufficient mixing, and the mixing time is 1-4 hours;

[0098] Step 3: Use Cr30Ni70 strip as welding skin, use alcohol to remove grease on the surface of Cr30Ni70 strip, and wrap the powder prepared in step 2 in the Cr30Ni70 strip through flux-cored wire drawing equipment. The aperture of the first drawing die is 2.6 mm;

[0099] Step 4: After the first drawing process is completed, the die aperture is reduced successively, and finally a flux-cored welding wire with a diameter of 1.2 mm is obtained;

[0100] Step 5: After the flux-cored welding wire is drawn, it is wound on the welding wire reel by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for standby use.

[0101] The nickel-based flux-cored welding wire prepared in Example 2 was used for TP347H / 12Cr1MoV dissimilar steel butt welding. After testing, the mechanical properties of the dissimilar steel welded joints were as follows: tensile strength 449 MPa, elongation after fracture 27%, and room temperature impact toughness 91 J.

[0102] The present invention provides a TP347H-12Cr1MoV welding wire for welding dissimilar materials and a preparation method thereof, which has the following beneficial effects compared with the prior art:

[0103] (1) In view of the difference in thermophysical properties between TP347H and 12Cr1MoV dissimilar steels, the present invention designs a nickel-based welding material with a linear expansion coefficient that is intermediate between the two types of steel for welding connection; the designed welding wire has Ni as its matrix, has good toughness, and a linear expansion coefficient that is intermediate between the above two types of steel, thereby effectively reducing the problem of large welding residual stress concentration caused by the difference in thermophysical properties between the dissimilar steels.

[0104] (2) In view of the composition difference between TP347H and 12Cr1MoV dissimilar steels, the present invention designs a Ni-Cr-Fe series of welding materials for connection. Since both TP347H and 12Cr1MoV steels are Fe-based, adding a certain amount of Fe element to the designed nickel-based welding material can ensure its excellent connection with the steels on both sides.

[0105] (3) Since TP347H / 12Cr1MoV dissimilar steels are used at high temperatures, a certain amount of Cr element is added to the weld skin of the welding wire of the present invention. Cr forms dense Cr2O3 oxide at high temperatures, so that the weld joint also has excellent high temperature resistance.

[0106] (4) The welding wire of the present invention is added with alloy elements of Mo, Nb, Ti and Re, which are dissolved in the nickel matrix to improve the toughness of the nickel-based weld. In addition, Mo can improve the high temperature resistance of the nickel-based weld to a certain extent.

[0107] (5) The welding wire developed by the method of the present invention has a small number of powder types and is convenient for large-scale production.

[0108] (6) The welding wire obtained by the present invention has a wire diameter of 1.2 mm and can be used for MAG / MIG welding as well as TIG welding, and has wide adaptability.

[0109] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A TP347H-12Cr1MoV welding wire for welding dissimilar materials, characterized in that: The welding wire comprises: a flux core and a welding skin; wherein the flux core comprises: 40-50% Fe powder; 10~15% powder; 5-10% Nb+Ta powder; 5-10% Mn powder; 1-2% Si powder; 1-2% Ti powder; 1-3% Re powder; The rest is Ni powder, and the sum of the mass percentages of the above components is 100%.

2. The TP347H-12Cr1MoV welding wire for dissimilar materials welding according to claim 1, characterized in that: The powder particle size in the medicine core is 100-200 meshes.

3. The TP347H-12Cr1MoV welding wire for dissimilar materials welding according to claim 2, characterized in that: The filling rate of the drug core is 20-22%.

4. The TP347H-12Cr1MoV welding wire for dissimilar materials welding according to any one of claims 1 to 3, characterized in that: The welding skin is Cr30Ni70 strip.

5. The TP347H-12Cr1MoV welding wire for dissimilar materials welding according to claim 4, characterized in that: The Cr30Ni70 strip has a thickness of 0.1 to 0.5 mm and a width of 5 to 10 mm.

6. A method for preparing the TP347H-12Cr1MoV welding wire for dissimilar materials welding as claimed in any one of claims 1 to 5, characterized in that: The method comprises: Weigh the powders according to mass percentage: Fe powder 40-50%, Mo powder 10-15%, Nb+Ta powder 5-10%, Mn powder 5-10%, Si powder 1-2%, Ti powder 1-2%, Re powder 1-3%, and the rest is Ni powder, and the sum of the mass percentages of the above components is 100%; The weighed drug powders are placed in a vacuum heating furnace for heating, and after drying, are placed in a powder mixer for mixing to obtain drug core powder; A Cr30Ni70 strip is used as a welding skin, and the flux core powder is wrapped in the Cr30Ni70 strip by a flux cored wire drawing device, and the welding wire is obtained by a drawing process.

7. The method according to claim 6, characterized in that The temperature of the heating treatment is 250-300° C. and the time is 1-4 hours.

8. The method according to claim 6, characterized in that The first drawing die aperture of the drawing process is 2.6 mm, and during the drawing process, the die aperture decreases successively.

9. The method according to claim 6, characterized in that The diameter of the welding wire is 1-1.5 mm.