ER70S-6 welding wire steel wire rod capable of reducing drawing wire breakage rate and manufacturing method of ER70S-6 welding wire steel wire rod
By optimizing the composition and process flow of ER70S-6 welding wire steel rod, the problems of high wire breakage rate and poor dimensional accuracy of finished products were solved, achieving low wire breakage rate and high-quality welding wire production to meet welding requirements.
Patent Information
- Application Number
- CN202411386689.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies result in a high wire breakage rate during the production of ER70S-6 welding wire rods, and poor control over the dimensional accuracy of finished products, which affects market competitiveness and welding quality.
By optimizing the composition design and process flow, including converter smelting, LF treatment, continuous casting, heating, rolling and cooling, the composition and temperature of molten steel are controlled, argon protection is used, and the rolling speed and cooling method are optimized to ensure the dimensional accuracy of the finished product, form a ferrite + pearlite structure, and reduce the risk of wire breakage during the drawing process.
It achieves low wire breakage rate and high finished product quality, stably controls N content below 40PPM, ensures finished product dimensions meet C-grade precision, and reduces the risk of wire breakage caused by uneven cross-sectional deformation.
Smart Images

Figure CN119016937A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-speed wire production, and specifically relates to an ER70S-6 welding wire rod steel with reduced wire breakage rate during drawing and a manufacturing method thereof. Background Art
[0002] ER70S-6 is a commonly used low alloy steel gas shielded welding wire, mainly used for welding carbon steel and 500MPa grade low alloy steel. This welding wire has good welding process performance, stable arc burning, less spatter, beautiful weld formation, low weld metal porosity sensitivity, good all-position welding process, and can be suitable for a wider welding current range. With the promotion of welding automation technology and the improvement of welding quality requirements, the market demand for ER70S-6 steel wire rod has been increasing year by year, and the market has reported the problem of ER70S-6 welding wire steel wire rod breaking during drawing. Therefore, the development of ER70S-6 welding wire steel wire rod with low wire breakage rate is an effective way to increase market competitiveness.
[0003] According to the current information, publication number CN114058819A proposes an ER70S-6 hot-rolled wire rod and a preparation method thereof, the technical scheme of which includes converter smelting, LF refining, continuous casting of a six-machine six-stream arc-shaped square billet continuous casting machine, heating by a regenerative heating furnace, high-pressure water dephosphorization, wire rolling, bundling, weighing, hanging and warehousing. Its advantage is that it adjusts the composition of the finished product, reduces the tensile strength of the wire rod, and increases the drawing performance of the wire rod. However, the process is cumbersome, the investment is large, and the dimensional accuracy of the finished product is not controlled. The control of the dimensional accuracy of the finished product is an important factor affecting the wire breakage rate in drawing.
[0004] Publication No. CN117548904A proposes a production method for stabilizing the performance of high-speed drawing welding wire ER70S-6, which includes: molten iron pretreatment, 100-ton top and bottom double-blowing converter, LF furnace refining, continuous casting, acceptance, loading, billet heating, high-pressure water descaling, rolling, controlled water cooling, diameter gauge, laying machine, Stelmor roller cooling, coiling, trimming, surface quality inspection, packaging, weighing, hanging, and warehousing. Its advantages are stable control of the superheat of the ladle and the dimensional accuracy of the product, but the finished product composition setting is loose, the composition is not designed in a targeted manner, the subsequent process is controlled by law, and there is still a great risk of breakage during the drawing process.
[0005] Publication No. CN118326109A discloses a method for reducing the wire breakage rate of ER70S-6 by controlling the nitrogen content in steel. The control method includes the following steps: converter smelting, deoxidation alloying, refining submerged arc slag making, and continuous casting protection pouring. The nitrogen content of the finished ER70S-6 welding wire steel wire rod produced by this method can be stably controlled to ≤50PPM, which reduces the wire breakage rate of ER70S-6 to a certain extent. However, this method only controls one of the factors affecting the wire breakage rate, and other factors are not mentioned.
[0006] Therefore, the present invention comprehensively approaches the known factors that affect the wire breakage rate during drawing, and improves the wire rod drawing performance and reduces the wire breakage rate during drawing of ER70S-6 welding wire steel by improving and controlling the composition design, converter smelting, LF treatment, continuous casting, heating, rolling, finished product finishing, cooling and other steps. Summary of the invention
[0007] The purpose of the present invention is to provide an ER70S-6 welding wire steel wire rod with a reduced wire breakage rate during drawing and a manufacturing method thereof. Through reasonable component composition, smelting control and rolling process coordination, an ER70S-6 welding wire steel wire rod with a low wire breakage rate during drawing and high product quality is produced.
[0008] The present invention is achieved through the following technical scheme: an ER70S-6 welding wire steel wire rod with reduced wire breakage rate during drawing, characterized in that it comprises the following components in mass percentage: C: 0.06-0.08%; Si: 0.80-0.88%; Mn: 1.40-1.48%; P: ≤0.015%; S: ≤0.015%; Al: ≤0.005%; Ca: ≤0.001%; O: ≤40PPM; N: ≤40PPM; Ni: ≤0.15%; Cr: ≤0.10%; Cu: ≤0.10%; Mo: ≤0.10%; V: ≤0.03%; Ti+Zr: ≤0.15%; the rest are Fe and unavoidable impurities.
[0009] The present invention also discloses a method for manufacturing the wire rod, which includes a molten iron pretreatment step, a converter smelting step, a LF treatment step, a continuous casting step, a heating step, a rolling step, a finished product finishing step, and a cooling step; and is characterized in that: The smelting steps are as follows: argon is blown at the bottom of the converter during the whole process of blowing, and no nitrogen-argon switching operation is performed. It is prohibited to add sintered ore or pelletized ore at the end of blowing or to purge nitrogen for temperature adjustment after blowing. Blowing end point control: C: ≤0.05%, P: ≤0.015%, steel tapping temperature: 1620℃-1650℃. After the steel tapping volume reaches 1 / 2, deoxidizer and alloy material are added. The order of adding alloys is: high silicon silicon manganese-silicon iron; aluminum iron, silicon calcium barium deoxidation is prohibited; after the alloy is added, 2.0-3.0kg / t (steel) of top slag is added; argon is blown during the whole steel tapping process; slag is blocked for steel tapping, and the amount of slag under the ladle is strictly controlled. In the later stage of steel tapping, long-term large argon stirring is avoided. Post-furnace target: C: ≤0.05%, Si: 0.74-0.84%, Mn: 1.34-1.44%, P: ≤0.015%, S: ≤0.018%, temperature: ≥1540℃. When the molten steel enters the LF furnace station, argon blowing and stirring are maintained. Lime and fluorite are added in batches to make slag. The amount of lime added is 3.2kg / t (steel). An appropriate amount of ferrosilicon powder is added for deoxidation, and the white slag time is maintained for not less than 15 minutes. Aluminum-containing materials and deoxidizers are prohibited during the treatment process, and calcium-containing materials are prohibited before steelmaking. No carbon is added when entering the station. For example, if the C in the refining process is ≥0.06%, no carbon increaser is added, C is controlled at 0.06-0.075%, and Mn is controlled at 1.44%. It is prohibited to add alloys during steelmaking or static blowing. The electrode power supply time T≤15min. After refining treatment in the LF furnace, it is prohibited to feed Ca wire, the net blowing time is ≥12min, and 40-60Kg of covering agent is added after static blowing. The continuous casting steps are as follows: during the casting process, argon-sealed long nozzles are used to protect the pouring, ensuring that the long nozzles are vertical and inserted to a depth of 150mm; the tundish superheat is controlled at 28±5°C, the continuous casting billet is produced with a cross section of 168mm*168mm, the process pulling speed is 2.1-2.3m / min, the pulling speed is maintained constant during the process, the crystallizer water flow is 120-140 m³ / h, the electromagnetic stirring current is 250A, the frequency is 3Hz, the tundish liquid level is maintained at ≥850mm, the tundish slag thickness is ≤150mm, the liquid slag layer thickness is 5-8mm, the nozzle insertion depth is 80-100mm, and the tundish type is selected as a plugger. The billet must be ensured to have no defects such as de-squareness and bulging that affect rolling; The rolling steps are as follows: the temperature of the soaking section of the billet entering the furnace is controlled at 1100-1150°C, the air-fuel ratio is 1.2±0.03 in the heating section and 1.0±0.05 in the soaking section, dephosphorization is used, and the dephosphorization water pressure is ≥16MPa. The temperature of the first finishing furnace is 880-930°C, the temperature of the second finishing furnace is 880-930°C, the spinning temperature is 860-890°C, the rolling speed is ≥100m / s, the starting speed of the air-cooled roller is ≤150mm / s, the fan is completely closed, the insulation cover is completely closed, the temperature of the wire rod entering the insulation cover is not lower than 750°C, and the target value of the temperature out of the insulation cover is 550±20°C. Increase the rolling speed and reduce the speed of the air-cooled roller. Increase the replacement frequency of the finished rollers, shortening the replacement of the finished rollers to once every 1.5 hours; The finished product finishing step is: cutting off the parts with different sizes and harmful defects, and there shall be no defects such as cracks, folds, ears, scars, delamination and inclusions; the size and shape shall be implemented according to the C-level precision in GB / T 14981-2009, and the allowable deviation of the finished product size is: ±0.15mm, and the out-of-roundness is: ≤0.24mm; The cooling step is as follows: the wire coils are stored in a warehouse for natural cooling and then centrally stacked.
[0010] Further: the structure is ferrite + pearlite, and the composition of the finished wire rod meets the requirements of AWS A5.18 / A5.18M:2021 standard.
[0011] The advantages of the present invention are: the ER70S-6 welding steel wire rod of the present invention stably controls N≤40PPM to reduce the drawing hardening rate of the wire rod, controls the temperature of each process in the rolling process to prevent the generation of abnormal tissue, and cooperates with the C-level control of the finished product size, which greatly reduces the risk of wire breakage caused by uneven cross-sectional deformation during the drawing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The microstructure of the ER70S-6 welding wire steel wire rod of the embodiment 15.5 mm invention (500X); Figure 2 The microstructure (500X) of the 26.5 mm inventive ER70S-6 welding wire steel wire rod of Example 1. DETAILED DESCRIPTION
[0013] The invention discloses an ER70S-6 welding wire steel wire rod with reduced wire breakage rate during drawing. The wire rod comprises the following components in percentage by mass: C: 0.06-0.08%; Si: 0.80-0.88%; Mn: 1.40-1.48%; P: ≤0.015%; S: ≤0.015%; Al: ≤0.005%; Ca: ≤0.001%; O: ≤40PPM; N: ≤40PPM; Ni: ≤0.15%; Cr: ≤0.10%; Cu: ≤0.10%; Mo: ≤0.10%; V: ≤0.03%; Ti+Zr: ≤0.15%; and the rest are Fe and unavoidable impurities.
[0014] The present invention also discloses a method for manufacturing the above-mentioned wire rod steel, which includes a molten iron pretreatment step, a converter smelting step, a LF treatment step, a continuous casting step, a heating step, a rolling step, a finished product finishing step, and a cooling step; wherein: The smelting steps: During the whole process of converter blowing, argon is blown from the bottom, and no nitrogen-argon switching operation is performed to prevent nitrogen addition to the molten steel. It is forbidden to add sintered ore or pelletized ore at the end of blowing or to purge nitrogen for temperature adjustment after blowing. Blowing endpoint control: C: ≤0.05%, P: ≤0.015%, tapping temperature: 1620℃-1650℃. After the tapping volume reaches 1 / 2, deoxidizer and alloy material are added to reduce the time for the molten steel to contact with air and absorb nitrogen after deoxidation. The order of adding alloys is: high silicon silicon manganese-silicon iron, and aluminum iron, silicon calcium barium deoxidation is prohibited; after the alloy is added, add top slag 2.0-3.0kg / t (steel); argon is blown throughout the tapping process; slag is blocked for tapping, and the amount of slag under the ladle is strictly controlled. In the later stage of tapping, long-term large argon stirring is avoided. Post-furnace targets: C: ≤0.05%, Si: 0.74-0.84%, Mn: 1.34-1.44%, P: ≤0.015%, S: ≤0.018%, temperature: ≥1540℃. The molten steel enters the LF furnace station and keeps blowing argon and stirring. Lime and fluorite are added in batches to make slag. The amount of white lime added is 3.2kg / t (steel). An appropriate amount of ferrosilicon powder is added for deoxidation. The white slag time is kept for not less than 15min. The use of aluminum-containing materials and deoxidizers is prohibited during the treatment process, and calcium-containing materials are prohibited before steelmaking. No carbon is added when entering the station. For example, C≥0.06% in the refining process, no carbon increase agent is added, C is controlled at 0.06-0.075%, and Mn is controlled at 1.44%. It is prohibited to add alloys during steelmaking or static blowing; the electrode power supply time T≤15min; after refining treatment in the LF furnace, it is prohibited to feed Ca wire, the net blowing time is ≥12min, and 40-60Kg of covering agent is added after static blowing.
[0015] The continuous casting steps are as follows: the casting process uses an argon-sealed long nozzle to protect the pouring, prevents the molten steel from contacting the air and absorbing nitrogen during the pouring process, ensures that the long nozzle is vertical, and the insertion depth is 150mm; the tundish superheat is controlled at 28±5℃, the continuous casting billet is produced with a 168mm*168mm section, the process pulling speed is 2.1-2.3m / min, the pulling speed is maintained constant during the process, the crystallizer water flow is 120-140m³ / h, the electromagnetic stirring current is 250A, the frequency is 3Hz, the tundish liquid level is maintained at ≥850mm, the tundish slag thickness is ≤150mm, the liquid slag layer thickness is 5-8mm, the nozzle insertion depth is 80-100mm, and the tundish type is a plugger. The billet must ensure that there are no defects such as de-squareness and bulging that affect rolling.
[0016] The rolling steps are as follows: the temperature of the soaking section of the billet is controlled at 1100-1150° C., the air-fuel ratio is 1.2±0.03 in the heating section and 1.0±0.05 in the soaking section, dephosphorization is put into use, and the dephosphorization water pressure is ≥16MPa. The first finishing temperature is 880-930℃, the second finishing temperature is 880-930℃, the spinning temperature is 860-890℃, the rolling speed is ≥100m / s, the starting speed of the air-cooled roller is ≤150mm / s, the fan is completely closed, the insulation cover is completely closed, the temperature of the wire rod entering the insulation cover is not less than 750℃, and the target temperature out of the insulation cover is 550±20℃; increase the rolling speed, increase the accumulation thickness of the wire coil on the air-cooled roller; reduce the speed of the air-cooled roller, extend the slow cooling time of the wire coil in the insulation cover, reduce the cooling rate, obtain sufficient ferrite + pearlite structure, reduce the tensile strength, increase the cross-sectional shrinkage, increase the replacement frequency of the finished product roller, shorten the replacement of the finished product roller to 1.5h, cut off the head and tail size tolerance parts, and the finished product size and shape meet the C-level accuracy in GB / T 14981-2009, accounting for more than 90% of the overall.
[0017] The finished product finishing steps are as follows: the parts with different sizes and harmful defects are removed, and there shall be no defects such as cracks, folds, ears, scars, delamination and inclusions; the size and shape are implemented in accordance with the C-level precision in GB / T 14981-2009, and the allowable deviation of the finished product size is: ±0.15mm, and the out-of-roundness is: ≤0.24mm.
[0018] The cooling step: the wire coils are put into the warehouse for natural cooling and then stacked. After stacking, insulation cloth is added and the vents are kept away.
[0019] The present invention is further described below by way of examples.
[0020] Example 1-2: Example 1 is ER70S-6 welding wire steel wire rod with a specification of 5.5 mm, and Example 2 is ER70S-6 welding wire steel wire rod with a specification of 6.5 mm. The components and parameters thereof are shown in the attached table.
[0021] According to the components and production method of the present invention, a 120-ton converter is used for smelting, and a 168mm*168mm cross-section slab is selected. The specific smelting process and slab composition are shown in Table 1 and Table 2: Table 1 Actual control of ER70S-6 smelting process in each embodiment Serial number Section of ingot (mm) Blowing end point C% Blowing end point P% Process pulling speed m / min Net blowing time min Superheat℃ Example 1 168*168 0.036 0.009 2.1 12 30 Example 2 168*168 0.043 0.011 2.2 12 30 The process drawing speed and superheat are stable, and the net blowing time is sufficient to prevent the billet from segregation, de-squareness and bulging.
[0022] Table 2 Actual composition of ER70S-6 smelted in each example Serial number C% Si% Mn% P% S% Al% Ca% N(PPM) Example 1 0.069 0.836 1.44 0.011 0.0089 0.003 0.0004 30 Example 2 0.064 0.866 1.46 0.014 0.0088 0.003 0.0003 36 Stable control of N≤40PPM reduces the wire rod drawing hardening rate.
[0023] According to the composition and production method of the present invention, the rolling is carried out using a SMS wire mill, and the rolling specifications are 5.5 mm and 6.5 mm. The specific process is shown in Table 3: Table 3 Actual rolling process of ER70S-6 in each embodiment Serial number Soaking section temperature ℃ Precise temperature ℃ Precision temperature ℃ Spinning temperature ℃ Rolling speed m / s Air cooling roller start speed mm / s Fan start status Insulation cover opening Example 1 1130 906 913 882 102 150 Close All Close All Example 2 1132 917 910 871 102 150 Close All Close All The temperature of each process in the rolling process meets the temperature setting range of the present invention, the rolling speed and the initial speed setting of the air-cooled roller meet the speed setting range of the present invention, the fan and the insulation cover are turned on in accordance with the setting of the present invention, and the product structure type is ferrite + pearlite, without any abnormality. Figure 1 , Figure 2 ,in, Figure 1 Medium structure type: ferrite (90%) + pearlite (10%), Figure 2 Medium structure type: ferrite (85%) + pearlite (15%).
[0024] Table 4 Actual performance of ER70S-6 welding steel wire rod Serial number Delivery Status Wire specification mm Lower yield strength MPa Tensile strength MPa Elongation after break % Sectional shrinkage% Example 1 Hot Rolling 5.5 407 535 31 81 Example 2 Hot Rolling 6.5 392 507 31 81 The physical properties are in accordance with the setting of the present invention.
[0025] Table 5 ER70S-6 welding wire steel wire rod finished product specifications Serial number Wire specification mm Large surface size (mm) Small face size mm Positive deviation mm Negative deviation mm Out of roundness mm Example 1 5.5 5.57 5.37 0.07 -0.16 0.20 Example 2 6.5 6.55 6.36 0.05 -0.14 0.19 The product dimensions all meet the C-level precision in GB / T 14981-2009 to avoid the deformation of the larger diameter parts being greater than other parts during the drawing process. Strong compression deformation will lead to uneven deformation of the entire cross-section and inconsistent degree of work hardening. At the same time, due to the increase in surface friction in the parts with large deformation, transverse cracks or fish-scale cracks are formed on the surface under the action of tensile stress, resulting in drawing fracture.
[0026] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A ER70S-6 welding wire steel wire rod with reduced wire breakage rate during drawing, characterized in that: The welding wire steel wire rod comprises the following components in percentage by mass: C: 0.06-0.08%; Si: 0.80-0.88%; Mn: 1.40-1.48%; P:≤0.015%; S: ≤0.015%; Al: ≤0.005%; Ca: ≤0.001%; O: ≤40PPM; N: ≤40PPM; Ni: ≤0.15%; Cr: ≤0.10%; Cu: ≤0.10%; Mo: ≤0.10%; V: ≤0.03%; Ti+Zr: ≤0.15%; the rest are Fe and unavoidable impurities.
2. A method for manufacturing ER70S-6 welding wire steel wire rod with reduced wire breakage rate as claimed in claim 1, comprising a molten iron pretreatment step, a converter smelting step, a LF treatment step, a continuous casting step, a heating step, a rolling step, a finished product finishing step, and a cooling step; characterized in that: The smelting steps are as follows: blowing argon gas at the bottom of the converter during the whole process of blowing; blowing endpoint control: C: ≤0.05%, P: ≤0.015%, steel tapping temperature: 1620℃-1650℃; adding deoxidizer and alloy material after the steel tapping reaches 1 / 2, and the order of adding alloys is: high silicon silicon manganese-silicon iron; using non-aluminum iron, silicon calcium barium deoxidizer for deoxidation; blowing argon gas during the whole process of steel tapping; slag blocking steel tapping; post-furnace target: C: ≤0.05%, Si: 0.74-0.84 %, Mn: 1.34-1.44%, P: ≤0.015%, S: ≤0.018%, temperature: ≥1540℃; when the molten steel enters the LF furnace station, keep blowing argon and stirring, add lime and fluorite in batches to make slag, add appropriate amount of ferrosilicon powder for deoxidation, and keep the white slag time not less than 15min; control 0.06-0.075%, Mn control 1.44%; net blowing time ≥12min, add 40-60Kg of covering agent after static blowing; The continuous casting step comprises: an argon-sealed long nozzle is used to protect the casting during the casting process, the superheat of the tundish is controlled at 28±5°C, the continuous casting billet is produced with a cross section of 168mm*168mm, the process pulling speed is 2.1-2.3m / min, the pulling speed is maintained constant during the process, the crystallizer water flow is 120-140 m³ / h, the electromagnetic stirring current is 250A, the frequency is 3Hz, the tundish liquid level is maintained at ≥850mm, the tundish slag thickness is ≤150mm, the liquid slag layer thickness is 5-8mm, and the nozzle insertion depth is 80-100mm; The rolling steps include: when the billet enters the furnace, the temperature of the soaking section is controlled to be 1100-1150°C, the air-fuel ratio is 1.2±0.03 in the heating section and 1.0±0.05 in the soaking section, dephosphorization is used, and the dephosphorization water pressure is ≥16MPa; the first finishing temperature is 880-930°C, the second finishing temperature is 880-930°C, the spinning temperature is 860-890°C, the rolling speed is ≥100m / s, the starting speed of the air-cooled roller is ≤150mm / s, the fan is completely closed, the heat preservation cover is completely closed, the temperature of the wire rod entering the heat preservation cover is not less than 750°C, and the target value of the temperature out of the heat preservation cover is 550±20°C; The cooling step is as follows: the wire coils are stored in a warehouse for natural cooling and then centrally stacked.
3. A method for manufacturing ER70S-6 welding wire steel wire rod with reduced wire breakage rate as claimed in claim 2, characterized in that: In the continuous casting step, the type of the tundish is a stopper rod tundish.
4. The method for manufacturing ER70S-6 welding wire steel wire rod with reduced wire breakage rate according to claim 2, characterized in that: The covering agent is lime.
5. The method for manufacturing ER70S-6 welding wire steel wire rod with reduced wire breakage rate according to claim 2, characterized in that: The finished product finishing steps are as follows: the parts with different sizes and harmful defects are removed, and there shall be no cracks, folds, ears, scars, delamination and inclusion defects; the size and shape shall be implemented in accordance with the C-level precision in GB / T 14981-2009, and the allowable deviation of the finished product size is: ±0.15mm, and the out-of-roundness is: ≤0.24mm.
6. The method for manufacturing ER70S-6 welding steel wire rod with reduced wire breakage rate according to claim 2, characterized in that: The structure of welding wire steel wire rod is ferrite + pearlite.