Forging and heat treatment method for deep groove ball bearing ring

Through the forging and heat treatment methods of deep groove ball bearing rings, the problem of low contact fatigue life at high speeds is solved. High-temperature rotary furnace and carbide refinement process are adopted to improve the fatigue resistance and dimensional stability of the bearings and extend the fatigue resistance and dimensional stability of the bearings. The service life of the equipment.

CN119017013APending Publication Date: 2024-11-26HARBIN BEARING GROUP CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411136963.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When using conventional heat treatment processes at high speeds, deep groove ball bearings have low contact fatigue life, which leads to early fatigue peeling, affecting the use of the equipment.

Method used

A method of forging and heat treatment of deep groove ball bearing rings, including cutting materials, preheating, final heat, forging, rolling and forming, refining treatment, stress removal and high-temperature tempering, heating through a high-temperature rotary furnace , carbide refining process and tempering treatment at 200-250°C ensure uniformity and dimensional stability of the forging process.

Benefits of technology

It effectively improves the contact fatigue life of the bearing, reduces the premature fatigue peeling phenomenon, extends the service life of the equipment, and prevents cracks and dimensional instability by refining the size and uniform distribution of carbide particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017013A_ABST
    Figure CN119017013A_ABST
Patent Text Reader

Abstract

The invention relates to a forging and heat treatment method for a deep groove ball bearing ring, in particular to a forging and heat treatment method for a deep groove ball bearing ring. The invention aims to solve the problems that when a conventional heat treatment process method is used for a deep groove ball bearing, due to the fact that the contact fatigue life of the bearing is short, the fatigue peeling phenomenon occurs in advance, and the use of instruments / equipment is affected. 2, preheating a material section; 3, final heating of the material sections; 4, forging the material sections; 5, ring rolling forming; (6) refining; seventhly, stress relief tempering is conducted; 8, high-temperature tempering treatment; and 9, heat treatment. By the adoption of the forging heat treatment method, the rated service life L10H of the bearing is 612 hours, and the rated service life L10H is prolonged by 1.61 times. The method is applied to the field of heat treatment processing of the ferrule for the deep groove ball bearing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging and heat treatment method for a deep groove ball bearing ring. Background Art

[0002] Deep groove ball bearings are the most widely used rolling bearings. They are characterized by low friction resistance and high speed. They can be used on instruments / equipment that bear radial loads, combined radial and axial loads, or axial loads, such as instruments, motors, household appliances, internal combustion engines, transportation vehicles, agricultural machinery, construction machinery, engineering machinery, etc.

[0003] Among them, deep groove ball bearings with an outer diameter of ≤150mm are the most widely used, and the most commonly used bearing ring is GCr15 high-carbon chromium bearing steel. If deep groove ball bearings within this size range are used for a long time on high-speed (speed > 5000r / min) instruments / equipment, using conventional heat treatment process methods, the bearings will have a low contact fatigue life and premature fatigue spalling, affecting the use of instruments / equipment. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that when using conventional heat treatment process methods for deep groove ball bearings, the bearings have a low contact fatigue life and premature fatigue spalling occurs, which affects the use of instruments / equipment. A forging and heat treatment method for deep groove ball bearing rings is provided.

[0005] The forging and heat treatment method of a deep groove ball bearing ring of the present invention is carried out according to the following steps:

[0006] 1. Cutting: Select hot-rolled bars for cutting to obtain material segments;

[0007] 2. Preheating of material section: preheating temperature: 820-860℃, holding time after color transparency 20-40min, protective atmosphere: nitrogen;

[0008] 3. Final heating of material section: Final heating is carried out after preheating, the heating temperature is 1050-1120℃, the insulation time after color is transparent is 10-20min, the protective atmosphere is nitrogen;

[0009] 4. Material segment forging: preheat the die before forging, use a forging press for forging, upsetting, forming, punching, the final forging temperature should be ≥950℃, and obtain a ring forging;

[0010] 5. Rolling forming: temperature measurement before rolling, rolling is carried out when the forging temperature is ≥900℃; if the forging temperature before rolling is <900℃, secondary heating is carried out, and rolling is carried out after heating is completed;

[0011] 6. Refining treatment: The forgings after rolling are placed in quenching oil for cooling. The quenching oil temperature is 60-100℃ and the cooling time is 2-5min. After the oil is discharged, hot cleaning is carried out. The cleaning temperature is 50-80℃ and the cleaning time is 2-5min.

[0012] 7. Stress relief tempering: Temper the cleaned forgings;

[0013] 8. High temperature tempering treatment: The forgings after step 7 are subjected to high temperature tempering treatment, the tempering temperature is 735-745°C, the tempering time is 3.5-4.5h, and then cooled to 500-600°C with the furnace, and then air-cooled to room temperature after being taken out of the furnace;

[0014] 9. Heat treatment: Turn, clean, dry, quench, cool, clean and prevent rust, foam and clean the forged parts after tempering. Finally, temper at 200-250℃ for 210-270min. The forging and heat treatment method of deep groove ball bearing ring is completed.

[0015] The beneficial effects of the present invention are:

[0016] 1. The bar material of the present invention is cut by a circular saw or a band saw, which ensures that the weight dispersion of the material section is controlled within ±5g, and the material section has no burrs, which can prevent forging folding crack defects or forging defects caused by large weight dispersion of the material section and burrs.

[0017] 2. The present invention uses a high-temperature rotary hearth furnace instead of a medium-frequency induction heating furnace to heat the material section, thereby ensuring uniform heating of the material section and preventing the occurrence of forging overburning defects.

[0018] 3. The present invention adds a high-temperature rotary hearth furnace for secondary heating treatment, which performs secondary heating on forgings with low temperature before rolling, thereby reducing rolling cracks caused by low temperature before rolling.

[0019] 4. The present invention adopts a carbide refinement process after rolling. The ring is cooled by oil after rolling to achieve a rapid cooling effect, thereby preventing the generation of network carbides. A tempering process at 300-400°C is adopted to eliminate the internal stress and high residual austenite content generated by oil cooling under high temperature conditions, thereby preventing the generation of cracks. The high-temperature tempering process refines the carbide particle size and makes the carbides evenly distributed.

[0020] 5. The present invention adopts a tempering temperature of 200-250° C. during heat treatment, which can reduce the residual austenite content in the ferrule after heat treatment to less than 5%, thereby ensuring the dimensional stability of the ferrule during subsequent processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1The metallographic structure of the 6210 outer ring after forging and quenching + stress relief tempering in Example 1 (1000×);

[0022] Figure 2 The metallographic structure of the 6210 outer ring after forging and high temperature tempering in Example 1 (1000×);

[0023] Figure 3 This is the quenched and tempered metallographic structure (1000×) of the 6210 outer ring after carbide refinement treatment in Example 1. DETAILED DESCRIPTION

[0024] Specific implementation method 1: In this implementation method, a forging and heat treatment method of a deep groove ball bearing ring is carried out according to the following steps:

[0025] 1. Cutting: Select hot-rolled bars for cutting to obtain material segments;

[0026] 2. Preheating of material section: preheating temperature: 820-860℃, holding time after color transparency 20-40min, protective atmosphere: nitrogen;

[0027] 3. Final heating of material section: Final heating is carried out after preheating, the heating temperature is 1050-1120℃, the insulation time after color is transparent is 10-20min, the protective atmosphere is nitrogen;

[0028] 4. Material segment forging: preheat the die before forging, use a forging press for forging, upsetting, forming, punching, the final forging temperature should be ≥950℃, and obtain a ring forging;

[0029] 5. Rolling forming: temperature measurement before rolling, rolling is carried out when the forging temperature is ≥900℃; if the forging temperature before rolling is <900℃, secondary heating is carried out, and rolling is carried out after heating is completed;

[0030] 6. Refining treatment: The forgings after rolling are placed in quenching oil for cooling. The quenching oil temperature is 60-100℃ and the cooling time is 2-5min. After the oil is discharged, hot cleaning is carried out. The cleaning temperature is 50-80℃ and the cleaning time is 2-5min.

[0031] 7. Stress relief tempering: Temper the cleaned forgings;

[0032] 8. High temperature tempering treatment: The forgings after step 7 are subjected to high temperature tempering treatment, the tempering temperature is 735-745°C, the tempering time is 3.5-4.5h, and then cooled to 500-600°C with the furnace, and then air-cooled to room temperature after being taken out of the furnace;

[0033] 9. Heat treatment: Turn, clean, dry, quench, cool, clean and prevent rust, foam and clean the forged parts after tempering. Finally, temper at 200-250℃ for 210-270min. The forging and heat treatment method of deep groove ball bearing ring is completed.

[0034] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that a circular saw or a band saw is used for cutting in step 1. The rest is the same as specific implementation method 1.

[0035] Specific implementation method three: This implementation method is different from the specific implementation method one in that a high-temperature rotary bottom heating furnace is used for preheating and final heating of the material segment. The rest is the same as the specific implementation method one.

[0036] Specific embodiment 4: This embodiment is different from specific embodiment 1 in that the temperature of mold preheating in step 4 is 150-250° C. and the preheating time is 15-20 minutes. The rest is the same as specific embodiment 1.

[0037] Specific embodiment 5: This embodiment is different from specific embodiment 1 in that the heating temperature of the second heating in step 5 is 950-1000° C. and the heating time is 10-15 min. The rest is the same as specific embodiment 1.

[0038] Specific implementation method 6: This implementation method is different from the specific implementation method 1 in that the tempering temperature in step 7 is 300-400° C. and the tempering time is 1-3 hours. The rest is the same as the specific implementation method 1.

[0039] Specific implementation method 7: This implementation method is different from specific implementation method 1 in that the cleaning in step 9 is divided into cleaning agent cleaning and water cleaning, the cleaning temperature is 50-80°C, and the cleaning time for each step is 3-6 minutes. The rest is the same as specific implementation method 1.

[0040] Specific implementation example eight: This implementation example is different from specific implementation example one in that the drying temperature of step nine is 100-150° C. and the drying time is 3-6 minutes. The rest is the same as specific implementation example one.

[0041] Specific embodiment 9: This embodiment is different from specific embodiment 1 in that the heating temperature of quenching in step 9 is 830-850° C. and the heating time is 35-60 min. The rest is the same as specific embodiment 1.

[0042] Specific embodiment 10: This embodiment is different from specific embodiment 1 in that the cooling in step 9 is firstly carried out by salt bath cooling and then by air cooling; wherein the salt temperature is 160-190°C, the water content in the salt bath is 0%-0.6%, the cooling time is 3-6 minutes, the air cooling time is 3-6 minutes, and the surface temperature of the ferrule after air cooling is ≤50°C. The rest is the same as specific embodiment 1.

[0043] The beneficial effects of the present invention are verified by the following experiments:

[0044] Example 1 Forging and heat treatment process of outer ring of deep groove ball bearing 6210

[0045] 1. Cutting

[0046] The raw materials are hot-rolled bars produced by Beiman Special Steel Co., Ltd., material: GCr15, diameter: 60mm, cut using a circular saw, section length: 45±0.5mm, burr-free, ensuring that the weight dispersion of the section is controlled within ±5g, and the cut surface is smooth and burr-free.

[0047] 2. Forging

[0048] 2.1 Preheating of material sections: Use a high-temperature rotary bottom heating furnace to preheat the material sections. Preheating temperature: 850℃, holding time after color transparency for 30 minutes, protective atmosphere: nitrogen. The material sections are heated independently in the rotary bottom heating furnace, first in first out.

[0049] 2.2 Final heating of material sections: Use a high-temperature rotary bottom heating furnace to final heat the material sections.

[0050] Into the high temperature rotary bottom heating furnace, heating temperature: 1100℃, heat preservation time after color transparent: 15min, protective atmosphere: nitrogen. The material sections are heated independently in the rotary bottom heating furnace, first in first out.

[0051] 2.3 Material segment forging: Forging is performed using a forging press. Before forging, the forging die of the forging press needs to be preheated at 150-250°C. The forging process is divided into: upsetting, forming, punching, and obtaining a ring forging. The final forging temperature is measured at 960°C using an infrared thermometer.

[0052] 2.4 Rolling forming: Since the outer ring of 6210 has a thin wall and cools down quickly, the temperature is measured by an infrared thermometer before rolling, and the temperature is 880℃. The forging is transferred to another high-temperature rotary bottom heating furnace for secondary heating. The secondary heating process is: heating temperature: 980℃, heating time: 12min. After the secondary heating is completed, the vertical rolling machine is used for rolling. After the rolling is completed, the temperature of the forging is measured by an infrared thermometer and is 910℃.

[0053] 2.5 Refining treatment: The forgings after rolling are directly put into the quenching oil for rapid cooling. The quenching oil temperature is 80℃ and the cooling time is 3 minutes. After the oil is discharged, hot cleaning is carried out. The cleaning temperature is 60℃ and the cleaning time is 3 minutes.

[0054] 2.6 Stress relief tempering: The cleaned forgings are tempered in a continuous mesh bag tempering furnace to eliminate the stress and high residual austenite produced by high temperature quenching. Tempering temperature: 350℃, tempering time: 2 hours.

[0055] 2.7 High temperature tempering treatment: Use a periodic box annealing furnace for high temperature tempering treatment, tempering temperature: 740℃, tempering time: 4 hours, then cool to 550℃ with the furnace, and then air cool to room temperature.

[0056] 3. Turning

[0057] Use a lathe to process forgings into workpieces of qualified size according to the process drawings.

[0058] 4. Heat treatment

[0059] The heat treatment (quenching and tempering) of the rings is processed using a salt bath martensitic quenching production line with a protective atmosphere roller hearth furnace.

[0060] 4.1 Pre-cleaning of the ring: Pre-cleaning removes impurities such as cutting fluid, dust, oil, etc. on the surface of the ring to ensure that the appearance color of the ring is consistent after quenching and tempering. The ring is placed on the tooling according to the process requirements and enters the pre-cleaning station, which is divided into cleaning agent cleaning and water cleaning. Cleaning temperature: 60°C, each cleaning time: 4.5min; drying after cleaning, drying temperature: 120°C, drying time: 4.5min. The cleaning agent is a water-based metal cleaning agent produced by Nanjing Kerun Industrial Media Co., Ltd., model: KR-F400H;

[0061] 4.2 Quenching heating: Heating temperature: 833℃, heating time: 40min.

[0062] 4.3 Cooling: Use salt bath cooling, the moving table moves up and down, and the salt tank stirring motor starts to improve the salt cooling performance. Salt temperature: 180℃, water content in the salt bath: 0%, cooling time: 4.5min.

[0063] 4.4 Air cooling: The air cooling time is 4.5 minutes. After air cooling, the surface temperature of the ring is ≤50℃.

[0064] 4.5 Cleaning and rust prevention: Immersion cleaning, a total of three stations: 1. Ultrasonic cleaning, frequency 28KHZ, water temperature 50℃; 2. Foaming cleaning, water temperature 50℃; 3. Cold water cleaning, water temperature 8℃, the cold water station contains a 0.6% mass fraction of sodium nitrite aqueous solution for rust prevention.

[0065] 4.6 Tempering: Use air tempering furnace for tempering. Tempering temperature: 230℃, tempering time: 240min.

[0066] Comparative Example 1: At present, deep groove ball bearing ring forging and heat treatment process methods:

[0067] 1. Cutting

[0068] The raw materials used are the same hot-rolled bars as in Example 1, and are cut using a fast shearing machine. Before cutting, the bars need to pass through a medium-frequency induction heating furnace to preheat the bars to 550-650°C. For each size of bar, a dedicated blade is used for cutting, and the weight dispersion of the material section is controlled within ±20g.

[0069] 2. Forging

[0070] 2.1 Material section heating: Use medium frequency induction heating furnace for heating, control the initial forging temperature, the material section furnace temperature is controlled at 1050℃~1120℃, and use infrared thermometer for temperature measurement.

[0071] 2.2 Material segment forging: Use a press or free forging for forging. Before forging, the forging die of the forging press needs to be preheated at 150-250℃, and the preheating time is 15 minutes. The forging process is divided into: upsetting, forming, punching, and obtaining a ring forging. The final forging temperature should be ≥900℃, and the final forging temperature is measured using an infrared thermometer.

[0072] 2.3 Rolling forming: Use a vertical rolling machine for rolling. Different types of forgings use different rolling dies. The temperature after rolling should be in the range of 850-950℃.

[0073] 2.4 Cooling: The rolled forgings fall onto a conveyor belt with fan cooling for air cooling. The cooling time is 2-4 minutes. After cooling, they fall into the material box.

[0074] 3. Annealing

[0075] Use a continuous spheroidizing annealing furnace for annealing. Place the forgings to be annealed into a tooling made of special heat-resistant steel. Annealing process: heating temperature: 780-800℃, heating time: 220-260min, fast cooling to 720℃ with the furnace, isothermal temperature 700-740℃, isothermal time 220-260min, slow cooling to 550℃ with the furnace, and air cooling to room temperature after being taken out of the furnace.

[0076] 4. Turning

[0077] Use a lathe to process forgings into workpieces of qualified size according to the process drawings.

[0078] 5. Heat treatment

[0079] The heat treatment (quenching and tempering) of the rings is processed using a salt bath martensitic quenching production line with a protective atmosphere roller hearth furnace.

[0080] 5.1 Pre-cleaning of the ring: Pre-cleaning removes impurities such as cutting fluid, dust, oil, etc. on the surface of the ring to ensure that the appearance color of the ring is consistent after quenching and tempering. The ring is placed on the tooling according to the process requirements and enters the pre-cleaning station, which is divided into cleaning agent cleaning and water cleaning. Cleaning temperature: 50-80℃, each cleaning time: 3-6min; drying after cleaning, drying temperature: 100-150℃, drying time: 3-6min.

[0081] 5.2 Cooling: Use salt bath cooling, the moving table moves up and down, and the salt tank stirring motor starts to improve the salt cooling performance. Salt temperature: 160-190℃, water content in the salt bath: 0%-0.6%, cooling time: 3-6min.

[0082] 5.3 Air cooling: The air cooling time is 3 to 6 minutes. After air cooling, the surface temperature of the ring is ≤50℃.

[0083] 5.4 Cleaning and rust prevention: Immersion cleaning, a total of three stations: 1. Ultrasonic cleaning, frequency 28 ~ 30KHZ, water temperature 40 ~ 60 ℃; 2. Foaming cleaning, water temperature 40 ~ 60 ℃; 3. Cold water cleaning, water temperature 6 ~ 10 ℃, the cold water station contains 0.5-0.8% concentration of sodium nitrite aqueous solution for rust prevention.

[0084] 5.5 Tempering: Use air tempering furnace for tempering. Tempering temperature: 160~190℃, tempering time: 210min~270min.

[0085] Figure 1 The metallographic structure (1000×) of the 6210 outer ring after forging and quenching + stress relief tempering in Example 1 is Figure 1 It can be seen that after the above process, the content of retained austenite in the ring is less than 5%. Figure 2 The metallographic structure (1000×) of the 6210 outer ring after forging, quenching + stress relief tempering + high temperature tempering. Figure 2 It can be seen that after the above process, the ring obtains fine dot-shaped and spherical pearlite (carbide refinement) structure. Figure 3 This is the quenched and tempered metallographic structure (1000×) of the 6210 outer ring after carbide refinement treatment. Figure 3 It can be seen that the carbide particles are fine and evenly distributed.

[0086] Compared with the comparative embodiment, the rod material of the embodiment is cut by a circular saw or a band saw, which ensures that the weight dispersion of the material segment is controlled within ±5g, and the material segment has no burrs, which can prevent forging folding crack defects or forging defects caused by large weight dispersion of the material segment and burrs.

[0087] Compared with the comparative example, the example uses a high-temperature rotary hearth furnace instead of a medium-frequency induction heating furnace to heat the material section, thereby ensuring the uniformity of heating the material section and preventing the occurrence of forging overburning defects.

[0088] Compared with the comparative embodiment, the embodiment adds a high-temperature rotary hearth furnace for secondary heating treatment, which performs secondary heating on the forgings with low temperature before rolling, thereby reducing rolling cracks caused by low temperature before rolling.

[0089] Compared with the comparative embodiment, the embodiment adopts a carbide refinement process after rolling, and the ring is quickly cooled by oil cooling after rolling to prevent the generation of network carbides; a tempering process of 300-400°C is adopted to eliminate the internal stress and high residual austenite content generated by oil cooling under high temperature conditions to prevent the generation of cracks; and the high-temperature tempering process is used to refine the carbide particle size and make the carbides evenly distributed.

[0090] Compared with the control example, the embodiment adopts a tempering temperature of 200-250° C. during heat treatment, which can reduce the residual austenite content in the ring after heat treatment to less than 5%, thereby ensuring the dimensional stability of the ring during subsequent processing.

[0091] After testing, the rated life L10H of the bearing in the comparative embodiment is 380 hours. Compared with the comparative embodiment, the rated life L10H of the bearing in Example 1 is 612 hours, and the rated life L10H is increased by 1.61 times.

Claims

1. A forging and heat treatment method for a deep groove ball bearing ring, characterized in that The method proceeds as follows:

1. Cutting: Select hot-rolled bars for cutting to obtain material segments; 2. Preheating of material section: preheating temperature: 820-860℃, holding time after color transparency 20-40min, protective atmosphere: nitrogen; 3. Final heating of material section: Final heating is carried out after preheating, the heating temperature is 1050-1120℃, the insulation time after color is transparent is 10-20min, the protective atmosphere is nitrogen; 4. Material segment forging: preheat the die before forging, use a forging press for forging, upsetting, forming, punching, the final forging temperature is ≥950℃, and a ring forging is obtained; 5. Rolling forming: temperature measurement before rolling, rolling is carried out when the forging temperature is ≥900℃; if the forging temperature before rolling is <900℃, secondary heating is carried out, and rolling is carried out after heating is completed; 6. Refining treatment: The forgings after rolling are placed in quenching oil for cooling. The quenching oil temperature is 60-100℃ and the cooling time is 2-5min. After the oil is discharged, hot cleaning is carried out. The cleaning temperature is 50-80℃ and the cleaning time is 2-5min.

7. Stress relief tempering: Temper the cleaned forgings; 8. High temperature tempering treatment: The forgings after step 7 are subjected to high temperature tempering treatment, the tempering temperature is 735-745°C, the tempering time is 3.5-4.5h, and then cooled to 500-600°C with the furnace, and then air-cooled to room temperature after being taken out of the furnace; 9. Heat treatment: Turn, clean, dry, quench, cool, clean and prevent rust, foam and clean the forged parts after tempering. Finally, temper at 200-250℃ for 210-270min. The forging and heat treatment method of deep groove ball bearing ring is completed.

2. A forging and heat treatment method for a deep groove ball bearing ring according to claim 1, characterized in that Step 1: Use a circular saw or band saw to cut the material.

3. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that A high-temperature rotary bottom heating furnace is used for preheating and final heating of the material sections.

4. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that Step 4: The mold preheating temperature is: 150-250°C, and the preheating time is 15-20 minutes.

5. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that Step 5: The heating temperature of the secondary heating is 950-1000°C and the heating time is 10-15 minutes.

6. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that Step 7: The tempering temperature is 300-400° C. and the tempering time is 1-3 hours.

7. A forging and heat treatment method for a deep groove ball bearing ring according to claim 1, characterized in that The cleaning in step nine is divided into cleaning agent cleaning and clean water cleaning, the cleaning temperature is 50-80°C, and the cleaning time for each step is 3-6 minutes.

8. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that The drying temperature of step nine is 100-150° C., and the drying time is 3-6 minutes.

9. The forging and heat treatment method of a deep groove ball bearing ring according to claim 1, characterized in that The heating temperature of the quenching in step nine is 830-850° C., and the heating time is 35-60 min.

10. A forging and heat treatment method for a deep groove ball bearing ring according to claim 1, characterized in that The cooling in step nine is first performed by salt bath cooling and then air cooling; wherein the salt temperature is 160-190°C, the water content in the salt bath is 0%-0.6%, the cooling time is 3-6 minutes, the air cooling time is 3-6 minutes, and the surface temperature of the ferrule after air cooling is ≤50°C.

Citation Information

Patent Citations

  • Strengthening and toughening thermal treatment method for hot-forging die of wearing plate

    CN102676778A

  • Rapid spheroidizing annealing process for bearing ring

    CN105543453A

  • Carbide superfine treatment technology for high-carbon chromium steel

    CN106868258A

  • Large-scale bearing ring workblank forming processing technology

    CN111774810A

  • Forging and heat treatment process for precise angular contact ball bearing ring

    CN117984055A