Manufacturing method of automotive trim injection-molded part

By adding metal organic skeleton material and bismuth strontium calcium copper compound composite catalyst to polypropylene material, low-pressure injection molding process is used to solve the uniformity and stability of complex component polypropylene automotive interior injection molding parts under low pressure conditions, reducing the problem of uniformity and stability of complex components of polypropylene automobile interior injection molding parts under low pressure conditions, The injection molding machine load is improved and the injection molding effect is improved.

CN119017629AInactive Publication Date: 2024-11-26ANHUI HONGYE PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411164635.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the injection molding process of automobile interior, how to effectively mold complex components of polypropylene materials under low pressure conditions to avoid the problems of uneven material distribution and excessive load of the injection molding machine.

Method used

By adding a catalyst formed by compounding metal organic framework material with bismuth strontium calcium copper to the polypropylene material, a low-pressure injection molding process is adopted to make the internal solid particles of the polypropylene evenly distributed and fully fused, reducing the injection molding pressure and improving the uniformity of the injection molding parts. and stability while reducing the load on the injection molding machine.

Benefits of technology

The uniformity and stability of injection molding parts in polypropylene automotive interiors are achieved, the load of the injection molding machine is reduced, the injection molding effect is significantly improved, and the inadequate integration of materials and safety hazards caused by high-pressure injection molding are avoided.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a manufacturing method of an automotive interior injection molded part, which comprises the following steps: uniformly mixing polypropylene, a polypropylene filler, a catalyst, a hardening agent, a stabilizer, a coloring agent and an auxiliary agent, adding the mixture into a granulator, stirring, heating, melting, granulating and cooling to prepare granular polypropylene master batch; feeding the polypropylene master batch into an injection molding machine, and performing low-pressure injection molding to prepare an injection molding blank; and the injection molding blank is subjected to deburring, polishing, cleaning and surface pattern treatment, and the automotive trim injection molding part is obtained. By adding the catalyst generated by compounding the metal organic framework material and the bismuth-strontium-calcium-copper compound, the injection molding pressure of the polypropylene automotive interior injection molding part can be reduced, and various solid particles in polypropylene are uniformly distributed and fully fused by adopting a low-pressure injection molding process, so that the injection molding effect is improved. Therefore, the uniformity and the stability of the automotive trim injection-molded part are remarkably improved, and meanwhile, the load of an injection molding machine can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing an automobile interior molding injection part, and belongs to the technical field of automobile parts injection molding processing. Background Art

[0002] Automotive interior parts include instrument panel accessories, seat accessories, floor accessories, roof panel accessories, steering wheel accessories, door interior accessories, rearview mirrors, etc.

[0003] According to the type of automobile interior plastics, there are PP, ABS, ABSPC, etc. Mostly used for dashboards, door inner panels are mostly made of PP, PPEPDM, ABS or PC / ABS, defogger grilles, handles, glove boxes are mostly made of ABS, PC / ABS or PP, and air-conditioning outlets are generally made of ABS, PC / ABS or PET.

[0004] Automotive interior parts are usually made by injection molding, which is performed using an injection molding machine. For polypropylene injection molding, the higher the injection pressure, the better the injection effect. If the pressure is too low, it will lead to poor injection and bubbles, which will cause safety hazards. In addition, if the injection pressure is too high, the injection speed may be too fast, making it impossible for the material to be fully integrated, and it will also increase the load on the machine.

[0005] Therefore, for polypropylene injection molding with fewer component types, the injection pressure is usually 500-1500psi. However, for high-performance automotive interior injection moldings with more component types, how to perform low-pressure injection molding is a difficult problem. Based on this, the present invention is proposed. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a method for manufacturing an automobile interior injection molded part. The specific technical solution is as follows:

[0007] A method for manufacturing an automobile interior injection molded part comprises the following steps:

[0008] Step 1: Granulation

[0009] The polypropylene, polypropylene filler, catalyst, hardener, stabilizer, colorant and additives are mixed evenly and added into a granulator, and then stirred, heated, melted, granulated and cooled to prepare granular polypropylene masterbatch;

[0010] Step 2: Injection molding

[0011] The polypropylene masterbatch is fed into the injection molding machine and low-pressure injection molding is adopted to form the injection-molded blank;

[0012] Step 3: Subsequent processing

[0013] The injection-molded blank is deburred, polished, cleaned, and surface patterned to obtain the automobile interior injection-molded part.

[0014] As a further improvement, in step 1, the mass ratio of the polypropylene, polypropylene filler, catalyst, hardener, stabilizer, colorant and additive is 80:(15-20):(0.7-0.9):(1-2):(0.1-0.2):(0.05-0.1):(0-5).

[0015] As a further improvement, the injection molding temperature in the injection molding machine is 190-200°C and the injection molding pressure is 300-360psi.

[0016] In a further improvement, the polypropylene filler is one or more of calcium carbonate and talcum powder.

[0017] In a further improvement, the hardener is a sorbitol nucleating agent.

[0018] In a further improvement, the stabilizer is a liquid calcium zinc stabilizer.

[0019] As a further improvement, the method for preparing the catalyst comprises the following steps:

[0020] 20 parts by weight of ZIF-8 metal organic framework material, 6 to 6.5 parts by weight of bismuth strontium calcium copper oxide and 6000 to 6500 parts by weight of ethanol are ultrasonically dispersed for 50 to 60 minutes to obtain a mixture; the mixture is reacted at a temperature of 80 to 83° C. for 34 to 36 hours. After the reaction is completed, the mixture is centrifuged, the filter residue is washed with ethanol, and then dried at a temperature of 70 to 75° C. to obtain a powdered catalyst.

[0021] As a further improvement, in step 1, the heating to the melting temperature is 164-167°C.

[0022] As a further improvement, the auxiliary agent is one or more of an anti-ultraviolet agent, a flame retardant, and an explosion-proof agent.

[0023] Beneficial effects of the present invention:

[0024] The method for manufacturing the automobile interior moldings of the present invention can reduce the injection molding pressure of polypropylene automobile interior moldings by adding a catalyst composited by a metal organic framework material and a bismuth strontium calcium copper compound, and adopts a low-pressure injection molding process so that various types of solid particles inside the polypropylene are evenly distributed and fully integrated with each other, thereby significantly improving the uniformity and stability of the automobile interior moldings and reducing the load of the injection molding machine. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] Example 1

[0027] Step 1: Granulation

[0028] 8 kg of polypropylene, 15 kg of calcium carbonate, 0.7 kg of catalyst, 1 kg of sorbitol nucleating agent, 0.1 kg of liquid calcium zinc stabilizer and 0.05 kg of colorant were mixed evenly and added into a granulator. After stirring, heating, melting, granulating and cooling, granular polypropylene masterbatch was prepared. The temperature for heating to melting was 164-167°C.

[0029] Step 2: Injection molding

[0030] The polypropylene masterbatch is fed into an injection molding machine and low-pressure injection molding is used to form an injection-molded blank; the injection molding temperature in the injection molding machine is 190-200° C., and the injection molding pressure is 300-320 psi.

[0031] Step 3: Subsequent processing

[0032] The injection-molded blank is deburred, polished, cleaned, and surface patterned to obtain the automobile interior injection-molded part.

[0033] The method for preparing the catalyst comprises the following steps:

[0034] 2 kg of ZIF-8 metal organic framework material, 0.6 kg of bismuth strontium calcium copper oxide and 600 kg of ethanol were ultrasonically dispersed for 50 minutes to obtain a mixture; the mixture was reacted at a temperature of 80-83°C for 34 hours. After the reaction was completed, it was centrifuged, the filter residue was washed with ethanol, and then dried at a temperature of 70°C to obtain a powdered catalyst.

[0035] Example 2

[0036] Step 1: Granulation

[0037] 8 kg of polypropylene, 18 kg of talcum powder, 0.8 kg of catalyst, 1.1 kg of sorbitol nucleating agent, 0.15 kg of liquid calcium zinc stabilizer, 0.07 kg of colorant and 0.5 kg of anti-ultraviolet agent were mixed evenly and added into a granulator. After stirring, heating, melting, granulating and cooling, granular polypropylene masterbatch was prepared; wherein, the temperature for heating to melting was 164-167°C.

[0038] Step 2: Injection molding

[0039] The polypropylene masterbatch is fed into an injection molding machine and low-pressure injection molding is used to form an injection-molded blank; the injection molding temperature in the injection molding machine is 190-200° C., and the injection molding pressure is 320-350 psi.

[0040] Step 3: Subsequent processing

[0041] The injection-molded blank is deburred, polished, cleaned, and surface patterned to obtain the automobile interior injection-molded part.

[0042] The method for preparing the catalyst comprises the following steps:

[0043] 2 kg of ZIF-8 metal organic framework material, 0.63 kg of bismuth strontium calcium copper oxide and 610 kg of ethanol were ultrasonically dispersed for 50 minutes to obtain a mixture; the mixture was reacted at a temperature of 80-83°C for 35 hours. After the reaction was completed, the mixture was centrifuged, the filter residue was washed with ethanol, and then dried at a temperature of 72°C to obtain a powdered catalyst.

[0044] Example 3

[0045] Step 1: Granulation

[0046] 8 kg of polypropylene, 20 kg of calcium carbonate, 0.9 kg of catalyst, 2 kg of sorbitol nucleating agent, 0.2 kg of liquid calcium zinc stabilizer and 0.1 kg of colorant were mixed evenly and added into a granulator. After stirring, heating, melting, granulating and cooling, granular polypropylene masterbatch was prepared. The temperature for heating to melting was 164-167°C.

[0047] Step 2: Injection molding

[0048] The polypropylene masterbatch is fed into an injection molding machine and low-pressure injection molding is used to form an injection-molded blank; the injection molding temperature in the injection molding machine is 190-200° C., and the injection molding pressure is 350-360 psi.

[0049] Step 3: Subsequent processing

[0050] The injection-molded blank is deburred, polished, cleaned, and surface patterned to obtain the automobile interior injection-molded part.

[0051] The method for preparing the catalyst comprises the following steps:

[0052] 2 kg of ZIF-8 metal organic framework material, 0.65 kg of bismuth strontium calcium copper oxide and 650 kg of ethanol were ultrasonically dispersed for 60 minutes to obtain a mixture; the mixture was reacted at a temperature of 80-83°C for 36 hours. After the reaction was completed, the mixture was centrifuged, the filter residue was washed with ethanol, and then dried at a temperature of 75°C to obtain a powdered catalyst.

[0053] Comparative Example 1

[0054] Compared with Example 1, this example only differs in the preparation method of the catalyst; the preparation method of the catalyst comprises the following steps:

[0055] 2 kg of ZIF-8 metal organic framework material and 0.65 kg of bismuth strontium calcium copper bismuth compound were mixed and ground to obtain the catalyst.

[0056] Comparative Example 2

[0057] Compared with Example 1, this example only differs in the catalyst; in this example, an equal mass of ZIF-8 metal organic framework material is used to replace the catalyst in Example 1, and the rest are the same.

[0058] Comparative Example 3

[0059] Compared with Example 1, this example only differs in the catalyst; in this example, an equal mass of bismuth strontium calcium copper oxide is used to replace the catalyst in Example 1, and the rest are the same.

[0060] Comparative Example 4

[0061] Step 1: Granulation

[0062] 8 kg of polypropylene, 15 kg of calcium carbonate, 1 kg of sorbitol nucleating agent, 0.1 kg of liquid calcium zinc stabilizer and 0.05 kg of colorant were mixed evenly and added into a granulator. After stirring, heating, melting, granulating and cooling, granular polypropylene masterbatch was prepared. The temperature for heating to melting was 164-167°C.

[0063] Step 2: Injection molding

[0064] The polypropylene masterbatch is fed into an injection molding machine and low-pressure injection molding is used to form an injection-molded blank; the injection molding temperature in the injection molding machine is 190-200° C., and the injection molding pressure is 300-320 psi.

[0065] Step 3: Subsequent processing

[0066] The injection molded blanks are deburred, polished, cleaned, and surface patterned to obtain automobile interior injection molded parts.

[0067] Comparative Example 5

[0068] Compared with the comparative example 4, the injection pressure in this example is 600-630psi.

[0069] 《Tin Immersion Test》

[0070] The automotive interior injection molded parts corresponding to Examples 1 to 3 and Comparative Examples 1 to 5 were cut into sample plates of 10×10×0.7 cm, and then the sample plates were immersed in a 185°C lead solder melt for 3 to 15 seconds until stratification bubbles appeared. For existing polypropylene injection molded parts, if various solid particles are evenly distributed in the polypropylene, it is not easy to stratify in the high-temperature lead solder melt. The stratification is usually in the area where a large number of solid particles are enriched, and a large number of solid particles will lead to uneven distribution.

[0071] The test results corresponding to Examples 1 to 3 and Comparative Examples 1 to 5 are shown in Table 1:

[0072] Table 1

[0073] Tin resistance Example 1 No delamination or bubbles within 15 seconds, the board surface softens Example 2 No delamination or bubbles within 15 seconds, the board surface softens Example 3 No delamination or bubbles within 15 seconds, the board surface softens Comparative Example 1 After 5s, stratification and a large number of bubbles appeared Comparative Example 2 After 3s, stratification and a large number of bubbles appear Comparative Example 3 After 4 seconds, stratification and a large number of bubbles appear Comparative Example 4 After 3s, stratification and a large number of bubbles appear Comparative Example 5 No delamination or bubbles within 15 seconds, the board surface softens

[0074] In the above embodiment, an auxiliary agent may be added according to the needs of the automobile interior injection molded part, and the auxiliary agent is one or more of an anti-ultraviolet agent, a flame retardant, and an explosion-proof agent.

[0075] The CAS number of the ZIF-8 metal organic framework material is 59061-53-9; the molecular formula of the bismuth strontium calcium copper compound is Bi2Ca2Cu2O9Sr2, CAS114901-61-0.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing an automobile interior injection molded part, characterized in that: The following steps are involved: Step 1: Granulation The polypropylene, polypropylene filler, catalyst, hardener, stabilizer, colorant and additives are mixed evenly and added into a granulator, and then stirred, heated, melted, granulated and cooled to prepare granular polypropylene masterbatch; Step 2: Injection molding The polypropylene masterbatch is fed into the injection molding machine and low-pressure injection molding is adopted to form the injection-molded blank; Step 3: Subsequent processing The injection-molded blank is deburred, polished, cleaned, and surface patterned to obtain the automobile interior injection-molded part.

2. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: In step 1, the mass ratio of the polypropylene, polypropylene filler, catalyst, hardener, stabilizer, colorant and additive is 80:(15-20):(0.7-0.9):(1-2):(0.1-0.2):(0.05-0.1):(0-5).

3. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The injection molding temperature in the injection molding machine is 190-200°C, and the injection molding pressure is 300-360psi.

4. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The polypropylene filler is one or more of calcium carbonate and talcum powder.

5. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The hardener is a sorbitol nucleating agent.

6. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The stabilizer is a liquid calcium zinc stabilizer.

7. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The preparation method of the catalyst comprises the following steps: 20 parts by weight of ZIF-8 metal organic framework material, 6 to 6.5 parts by weight of bismuth strontium calcium copper oxide and 6000 to 6500 parts by weight of ethanol are ultrasonically dispersed for 50 to 60 minutes to obtain a mixture; the mixture is reacted at a temperature of 80 to 83° C. for 34 to 36 hours. After the reaction is completed, the mixture is centrifuged, the filter residue is washed with ethanol, and then dried at a temperature of 70 to 75° C. to obtain a powdered catalyst.

8. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: In step 1, the heating is performed to a melting temperature of 164 to 167°C.

9. The method for manufacturing an automobile interior molding according to claim 1, characterized in that: The auxiliary agent is one or more of an anti-ultraviolet agent, a flame retardant, and an explosion-proof agent.