Optimization method for pre-curing of wind power blade web

By heating and temperature control in advance during the resin infusion process of wind power blade webs, the exothermic peak temperature is reduced, the core material burning problem is solved, product quality and production efficiency are improved, and the precuring process of wind power blade webs is optimized.

CN119017740AActive Publication Date: 2024-11-26SINOMA TECH (YULIN) WIND POWER BLADE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411376552.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-26
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

During the resin curing process, wind power blade webs are prone to burning the core material due to the high exothermic peak temperature. The existing solutions require frequent detection and adjustment of the process to avoid this problem, but will extend the precuring cycle and affect production efficiency.

Method used

When the resin infusion amount reaches 1/3 to 2/3, the mold temperature is raised to 55 to 65°C, and the resin is heated in advance to cure the resin, reduce the exothermic peak temperature, and adjust it to 70 to 80°C after the exothermic peak is over. Perform insulation and curing to ensure temperature control of the curing process.

Benefits of technology

Effectively prevent the core material from burning, shorten the web curing time, improve product quality, optimize production processes, reduce the probability of secondary problems such as high-temperature damage of vacuum films, and improve production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017740A_ABST
    Figure CN119017740A_ABST
Patent Text Reader

Abstract

The invention discloses an optimization method for precuring a wind power blade web, which comprises the following steps: in a resin infusion molding process in a web manufacturing process, when the resin infusion amount is 1 / 3-2 / 3 of the total infusion amount, raising the temperature of a mold to 55-65 DEG C, maintaining the temperature to complete infusion, and after the exothermic peak of the resin is finished, adjusting the temperature of the mold to 70-80 DEG C for heat preservation and curing. According to the optimization method, on the premise that the production cycle is not affected, the exothermic peak temperature in the web curing process can be effectively reduced, the core material burning defect existing in the prior art is overcome, the occurrence probability of secondary problems such as vacuum film high-temperature damage caused by high temperature is reduced, the product quality of the wind power blade is remarkably improved, and the production cost is reduced. The production process flow is optimized, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of production of a wind turbine blade web, and in particular to an optimization method for pre-curing a wind turbine blade web. Background Art

[0002] Wind turbine blades are one of the core components of wind turbine generator sets, and their quality is directly related to the performance and efficiency of wind turbines. The structural components of wind turbine blades usually include outer shells, main beams and webs, among which the webs, as key structures, play the role of supporting the main beams and transmitting shear forces. The production of wind turbine blades in the industry usually includes two processes: pre-curing and post-curing. Pre-curing is the curing after resin infusion in the web manufacturing process, which is the web forming process; post-curing is the insulation curing process after the shell and components are bonded. The webs used in existing wind turbine blades are mainly composed of plies (i.e. fiber reinforced materials) and core materials, and are formed by vacuum infusion resin process. The production process usually includes the following steps: laying of outer skin cloth layers, laying of core materials, laying of inner skin cloth layers, arrangement of infusion auxiliary materials, vacuum packing, etc. Since the resin curing reaction is an endothermic reaction, it is necessary to heat the resin first to accelerate the curing of the resin. Therefore, the existing web curing process is to open the mold and preheat it to 40°C when the web is laid to the beginning of the auxiliary material arrangement, maintain this temperature for vacuum infusion, and after all the resin is infused, the mold is heated to 80°C for heat preservation and curing to complete the web pre-curing. However, since a large amount of heat is released during the resin curing process, the heat released by the resin will reach its peak during the process of resin heating and curing to the exothermic peak, and because there is a lot of resin in the infusion flow channel, it is easy to generate heat accumulation in the flow channel area, resulting in the core material burning exceeding the highest heat resistance temperature, and secondary problems such as high temperature causing the product to be unqualified. In actual production, in order to avoid the problem of core material burning during the resin curing process, multiple sampling points need to be frequently tested, and when the local temperature is too high, spraying or ice compressing is used to cool down. Not only is the operation complicated, it increases the workload and production cost, but also affects the product. To optimize production, people have tried to divide resin exotherm and resin curing into two stages through temperature control. That is, after the infusion is completed, the temperature is first adjusted to 65°C, and then the temperature is raised to 70-80°C for insulation and curing after the exothermic peak ends. Although this adjustment can solve the problem of core material burning caused by the exothermic peak, it will extend the pre-curing cycle and affect the overall production. Summary of the invention

[0003] In order to solve the defect of web pre-curing that easily causes core material to burn in existing production, the present invention provides an optimization method for pre-curing of wind turbine blade webs, which adopts the process of early heating and heat preservation to make the resin absorb heat in advance, thereby effectively preventing the core material from burning due to the high heat release temperature of the resin, thereby improving product quality. At the same time, the optimized process has no effect on the web forming cycle.

[0004] The optimized method for pre-curing the web of a wind turbine blade of the present invention is to increase the mold temperature to 55-65°C during the resin infusion molding step in the web manufacturing process when the resin infusion volume reaches 1 / 3-2 / 3 of the total infusion volume, maintain this temperature to complete the infusion, and adjust the mold temperature to 70-80°C for heat preservation and curing after the resin exothermic peak ends.

[0005] By preheating the resin when the resin infusion volume reaches 1 / 3 to 2 / 3, the resin flow rate is accelerated and the resin is cured in advance by endothermic curing, which speeds up the release of heat in the initial stage of curing. The process temperature range is set for different stages in the web curing process to reduce the exothermic peak temperature, thereby effectively preventing the core material from burning due to the high exothermic temperature of the resin. At the same time, the optimized process has no obvious change in the web pre-curing time, eliminating the impact of process adjustments on the web molding production cycle, thereby ensuring the smooth progress of the overall production.

[0006] As a limitation of the above technical solution, the auxiliary material arrangement process is preheated to 35-45° C. at the beginning, and the resin is poured to 1 / 3-2 / 3 of the total pouring volume while maintaining this temperature.

[0007] As a limitation of the above technical solution, the temperature is controlled by determining the end time of the resin exothermic peak through detection.

[0008] As a limitation of the above technical solution, the overall perfusion time is shortened to 50 to 60 minutes.

[0009] The pre-curing operating conditions of the web manufacturing process are further defined to optimize the web quality and process flow.

[0010] At the same time, the present invention also provides a wind turbine blade web, which is prepared by the above-mentioned optimization method.

[0011] As a limitation of the above technical solution, the web has no core material burnt defect.

[0012] The optimization method for pre-curing the web of a wind turbine blade of the present invention can effectively reduce the exothermic peak temperature of the web curing process, solve the core material burnout defect existing in the existing production, reduce the probability of secondary problems caused by the high temperature in the existing process such as high-temperature breakage of the vacuum membrane, significantly improve the product quality of wind turbine blades, optimize the production process flow, and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 , making a mold for the web of the present invention;

[0014] In the figure, 1-mold, 2-outer skin cloth layer, 3-core material, 4-inner skin cloth layer, 5-integrated guide net, 6-flow channel. DETAILED DESCRIPTION

[0015] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] The raw materials involved in the following examples and comparative examples are typical products purchased from the market.

[0017] Example

[0018] The production operations of the wind turbine blade web are as follows.

[0019] 1. Belly plate production

[0020] The production process is as follows: laying of outer skin layer, laying of core material, laying of inner skin layer, arrangement of infusion auxiliary materials, vacuum packing, etc. Figure 1 As shown,

[0021] (1) Laying out the outer skin fabric layer 2: Laying out the glass fiber fabric layer into the web mold 1 as the outer skin fabric layer 2 according to the process requirements;

[0022] (2) Laying the core material 3: Lay the core material 3 on top of the outer skin fabric layer 2 as required, and lay it in a fixed area;

[0023] (3) Laying the inner skin fabric layer 4: Laying the glass fiber fabric layer on the core material 3 as the inner skin fabric layer 4 according to the process requirements;

[0024] (4) Arrangement of pouring auxiliary materials: Arrange auxiliary materials such as release cloth, integrated guide net 5, runner 6, etc. according to process requirements;

[0025] (5) Vacuum packing: A vacuum packing operation is performed using a vacuum film and an exhaust system to create a negative pressure inside the web mold 1 as a whole for injecting the infusion resin.

[0026] 2. Web pre-curing

[0027] (1) Infusion and heating process

[0028] At the beginning of the auxiliary material arrangement process, the mold is heated to 35-45°C to keep the mold in a balanced temperature and suitable for infusion. The resin is infused at 35-45°C to stabilize the resin flow rate through temperature control. When the infusion reaches about 1 / 3 to 2 / 3 of the total resin infusion volume, the mold heating temperature is adjusted from 35-45°C to 55-65°C, and the subsequent resin infusion is maintained at 55-65°C. The infusion rate is improved, which not only shortens the infusion time to 50-60 minutes, but also starts the curing reaction in advance during the infusion process.

[0029] The viscosity and flow rate of the resin are directly related to the temperature. Increasing the infusion temperature during the infusion process will directly change the infusion flow rate and the wetting effect of the resin and the core material. Since the resin curing reaction process is an endothermic reaction, raising the temperature in advance will allow the resin to start reacting in advance and increase the temperature increase reaction rate. At the same time, the resin curing reaction process releases heat, providing heat for the resin curing, allowing the curing reaction to proceed in advance.

[0030] (2) Exothermic peak process

[0031] The total heat released during the overall curing process of the resin remains unchanged. The temperature is raised in advance during the resin infusion stage so that the heat of the curing reaction begins to be released during the heating process. This can effectively alleviate the concentrated release of heat from the exothermic peak, reduce the temperature in the flow channel area, effectively avoid the defect of core material burning, and improve the quality of the blade.

[0032] (3) Insulation and curing process

[0033] After the exothermic peak is over, the mold heating temperature is adjusted from 55-65℃ to 70-80℃ for heat preservation and curing. Due to the early temperature rise in the infusion stage, the infusion time is reduced, and the curing process is started in advance. After the exothermic peak is over, the mold temperature is raised to 70℃-80℃ to accelerate the heat preservation and curing process of the web, eliminate the impact on the web forming cycle, and keep the overall curing cycle of the web stable.

[0034] The web pre-curing process data is detailed in Table 1.

[0035] Table 1

[0036]

[0037] Comparative Example 1

[0038] This comparative example is a web manufacturing process before optimization, and its difference from the embodiment lies in the operation of the web pre-curing process, which is specifically as follows: when the web auxiliary materials are arranged, the mold is opened and preheated to 40°C, and this temperature is maintained to complete vacuum infusion, and the infusion time is 60 to 70 minutes. After all the resin infusion is completed, the mold temperature is raised to 80°C for insulation and curing. During the curing process, thermal imaging is used to measure the temperature of the product surface. If the temperature is greater than 50°C, it is circled with a marker, and a spray bottle is used to continuously spray ice water to cool the area with a temperature greater than 50°C; when the surface temperature of the product is higher than 60°C during the heating process, the insulation cotton is opened. Once the temperature is too high, spraying or ice compressing is used to cool it down until the web pre-curing is completed. The pre-curing time is 5.5 to 6 hours. The obtained web product is tested and the number of burnt defects of a single core material is 9.

[0039] Comparative Example 2

[0040] In this comparative example, based on the existing web manufacturing process (same as comparative example 1), the preheating temperature and the heat preservation and curing temperature are adjusted. The specific adjustment data are shown in Table 2.

[0041] Table 2

[0042]

[0043]

[0044] Comparative Example 3

[0045] In this comparative example, the web pre-curing process is adjusted. The specific operation is as follows: when the web auxiliary materials are arranged, the mold is opened and heated to 40°C, and this temperature is maintained for infusion to complete vacuum infusion, and the mold is adjusted to be heated to 65°C. After 4 hours, the exothermic peak ends, and then the mold is adjusted to be heated to 80°C for insulation and curing for 2.5 hours to complete the web pre-curing. The pre-curing time is 6.5 hours. The number of burnt defects of a single core material in the obtained web product is 1 after testing, but the pre-curing period is extended compared with the previous conventional process of 5.5 to 6 hours, which affects the overall production.

[0046] It can be seen from the comparative results that the adjustment of the infusion temperature will directly affect the resin flow rate, thereby changing the infusion time; increasing the infusion temperature will also affect the pre-curing time, thereby affecting product quality and other production conditions.

[0047] In summary, the optimization method of the present invention adjusts the web pre-curing process, that is, the mold is heated to 55-65°C when the web resin infusion volume is 1 / 3-2 / 3, so that the curing process is carried out in advance, the resin exotherm process is prolonged, and the concentrated heat release of the resin during the exotherm peak is effectively controlled to avoid the core material under the infusion flow channel being burned due to too high temperature. After the exotherm peak ends, the mold temperature is increased to 70°C-80°C to accelerate the web insulation curing process, and at the same time eliminates the influence of process adjustment on the web forming cycle, which not only significantly improves the product quality of wind turbine blades, but also optimizes the production process and improves production efficiency.

Claims

1. An optimization method for pre-curing a web of a wind turbine blade, characterized in that: In the resin infusion molding process of the web manufacturing process, when the resin infusion volume reaches 1 / 3 to 2 / 3 of the total infusion volume, increase the mold temperature to 55 to 65°C, maintain this temperature to complete the infusion, and after the resin exothermic peak ends, adjust the mold temperature to 70 to 80°C for heat preservation and curing.

2. The optimization method for pre-curing the web of a wind turbine blade according to claim 1, characterized in that: At the beginning of the auxiliary material placement process, preheat to 35-45°C and maintain this temperature to infuse the resin to 1 / 3-2 / 3 of the total infusion volume.

3. The optimization method for pre-curing the web of a wind turbine blade according to claim 1, characterized in that: The end time of the resin exothermic peak is determined by detection to control the temperature.

4. The optimization method for pre-curing the web of a wind turbine blade according to claim 1, characterized in that: The infusion time was shortened to 50-60 minutes.

5. A wind turbine blade web, characterized in that: The product is prepared by the optimization method described in any one of claims 1 to 4.

6. The wind turbine blade web according to claim 5, characterized in that: The web has no core material burnt defects.

Citation Information

Patent Citations

  • Manufacturing method of blade root prefabricated part of wind blade

    CN108943771A

  • Solution method for internal stress whitening

    CN109203513A

  • Blade forming method and blade

    CN114654765A

  • Intelligent pressure vacuum assisted staged resin infusion forming device and method

    CN118578692A