Film for battery bag and storage method thereof
By using sealing layer, metal layer and outer layer structure in the battery bag film, combined with specific storage temperature to control the flow and aggregation of smoothing agent, the problem of excessive flow and aggregation of smoothing agent at high temperatures is solved, and high molding is achieved Improvement of performance and process efficiency.
Patent Information
- Application Number
- CN202410648254.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-09
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The existing battery bag film can easily cause excessive smoothing agent to flow out at high temperatures, resulting in a decrease in process efficiency and a decrease in moldability, and it is difficult to prevent smoothing agent from aggregating, affecting product reliability.
The battery bag film with sealing layer, metal layer and outer layer structure is used to control the effluent and aggregation of smoothing agent by adjusting the storage temperature between 48°C and 57°C, ensuring that the surface roughness of the film is between Rt 13 μm and 20 μm and Rz 10 μm to Within the 15μm range, reduce excessive smoothing agent outflow and prevent aggregation.
After 30 days of storage, the size of the aggregation particles of the film surface smoothing agent decreased, the friction coefficient was maintained between 0.15 and 0.5, and the moldability reached 15mm to 25mm, improving process efficiency and product reliability.
Smart Images

Figure CN119017790A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a film for a battery bag and a method for preserving the same.
[0002] Cross-reference to related applications
[0003] This application claims priority to Korean Patent Application No. 10-2023-0066379 filed on May 23, 2023 and Korean Patent Application No. 10-2024-0061080 filed on May 9, 2024, the contents of which are incorporated herein by reference in their entirety.
[0004] Explanation of national support for R&D
[0005] This research was carried out through the following national projects.
[0006] -Department name: Ministry of Trade, Industry and Energy; Project management (specialized) organization name: Korea Institute of Industrial Technology Evaluation and Management; Research project name: Material and accessories packaging type (leading enterprise); Research project name: Development of a new generation of secondary battery bags that can achieve more than twice the high bonding strength (60°C); Project execution organization name: Yulchon Chemical Co., Ltd.; Project number: 20022450; Project unique number: 1415185612 Background Art
[0007] Generally, compared with cylindrical or prismatic batteries, pouch-type batteries used in electric vehicles and the like have the advantages of being easy to change shape and having high energy density. As an external material for wrapping the battery pack and electrolyte of the battery, the battery pouch must meet the required properties such as the bonding force between the layers composed of metal film and polymer, heat welding strength, electrolyte resistance, airtightness, moisture permeability, and formability. In particular, in order to apply the battery pouch to large batteries such as electric vehicles (EVs) and energy storage devices (ESS), high forming properties must be maintained. Therefore, the battery pouch must contain a lubricant (slip agent) as an additive to improve formability. The lubricant will flow out to the outermost surface of the bag to provide formability according to temperature and pressure. However, if too much lubricant flows out, the lubricant particles will agglomerate and cause process contamination, resulting in a sharp drop in process efficiency. Therefore, it is necessary to develop a battery pouch film that can prevent the lubricant from agglomerating while providing high formability. Summary of the invention
[0008] The technical problem of the present disclosure is to provide a battery pouch film with excellent moldability and reduced outflow of a lubricant, and a method for preserving the same.
[0009] One embodiment of the present disclosure provides the following battery bag film, which includes: a sealing layer containing a lubricant; a metal layer formed on the sealing layer; and an outer layer formed on the metal layer, after the film is stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black bag with a matt black appearance and an outer layer made of nylon is used to rub the outer surface of the black bag and the sealing layer or outer layer of the film at a speed of 400mm / 10s, the surface roughness value of the part where the lubricant flowing out of the film adheres to and forms a white band on the black bag satisfies Rt 13μm to 20μm and Rz 10μm to 15μm.
[0010] Still another embodiment of the present disclosure provides a battery pouch including the above-mentioned film for a battery pouch.
[0011] Another embodiment of the present disclosure provides a method for preserving the battery pouch film of the present disclosure, comprising the step of preserving the film at a temperature of 48° C. to 57° C.
[0012] According to an embodiment of the present disclosure, after manufacturing the battery bag film, the storage temperature can be adjusted to minimize the phenomenon of excessive outflow of the lubricant to the surface while containing a small amount of lubricant, thereby improving the efficiency of the lubricant. Therefore, the film of the present disclosure can prevent excessive outflow of the lubricant while exhibiting excellent formability, thereby preventing process defects caused by the lubricant. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The results of measuring the surface roughness of Examples 1 and 2 and Comparative Example 4 in Test Example 1 are shown.
[0014] Figure 2 This is an image of the lubricant inspection device used in Test Example 2.
[0015] Figure 3 This is an image of a black bag taken after the lubricant inspection in Test Example 2.
[0016] Figure 4 Graph showing lubricant inspection evaluation criteria (S, A, B grades) in Test Example 2.
[0017] Figure 5A The results of particle size analysis (80x image) of particles formed by agglomerating the lubricant in Example 1 (storage temperature 50° C.) after the lubricant inspection in Test Example 2 are shown.
[0018] Figure 5B The results of the size analysis of particles formed by agglomerating the lubricant in Example 1 (storage temperature 50° C.) after the lubricant inspection in Test Example 2 are shown (450-fold magnification image).
[0019] Fig. 6A The results of particle size analysis (80x image) of particles formed by agglomerating the lubricant in Comparative Example 4 (storage temperature 45° C.) after the lubricant inspection in Test Example 2 are shown.
[0020] Figure 6B The results of particle size analysis (450x image) of particles formed by agglomerating the lubricant in Comparative Example 4 (storage temperature 45° C.) after the lubricant inspection in Test Example 2 are shown. DETAILED DESCRIPTION
[0021] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings.
[0022] The multiple embodiments of the present disclosure disclosed in the specification are only for illustration, and the multiple embodiments of the present disclosure can be implemented in multiple implementations, and the present disclosure is not limited to the multiple embodiments described in the specification. The present disclosure can be implemented in multiple ways to form multiple implementations, and the multiple embodiments are not used to limit the present disclosure to specific disclosed implementations, and should be understood to include all changes, equivalent technical solutions, and alternative technical solutions within the concept and technical scope of the present disclosure.
[0023] Unless otherwise clearly indicated in the context, the expression in the singular includes the expression in the plural. In this application, the terms "including" or "having" are only used to specify the existence of the features, numbers, steps, actions, structural elements, components or their combinations described in the specification, and do not exclude the existence or additional possibility of one or more other features or numbers, steps, actions, structural elements, components or their combinations.
[0024] In this specification, the term "cell" means a battery, and has the broadest meaning to include various batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.
[0025] In this specification, "cell pouch" is formed by immersing battery structural elements such as a positive electrode, a negative electrode and a separator in an electrolyte. In order to accommodate the above-mentioned battery structural elements, it means the broadest meaning of processing a laminated structure film taking into account gas barrier properties, flexibility, electrolyte resistance and thermal adhesion into a bag or box shape.
[0026] In this specification, "formability" means the property that the battery bag film can be processed into a desired shape without cracking or breaking and can maintain its shape when processed into a specified shape. For example, the above-mentioned formability can be evaluated by applying a pressure of 0.3MPa to a test piece of the cut battery bag film to form it into a cup shape and measuring the maximum depth without cracking or breaking. More specifically, if all 10 of 10 identical film test pieces are not broken, a deeper depth can be used. If one breaks, the previous depth can be defined as the maximum height. For example, the above-mentioned formability evaluation can be evaluated by using a molded cup in the shape of a regular hexahedron (cup mouth size: 16cm×9cm). More specifically, it can be evaluated by the GS-S5 model of GWANGSHIN Hi-Tech.
[0027] One embodiment of the present disclosure relates to a battery bag film including a sealing layer, a metal layer formed on the sealing layer, and an outer layer formed on the metal layer, the sealing layer containing a lubricant, and after the film is stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black pouch with a matt black appearance and an outer layer made of nylon is used to rub the outer surface of the black pouch and the sealing layer or the outer layer of the film at a speed of 400mm / 10s, the surface roughness value of the part where the lubricant flowing out of the film adheres to and forms a white band on the black pouch reaches Rt 13μm to 20μm and Rz 10μm to 15μm.
[0028] According to one embodiment of the present disclosure, the film is stored at a temperature of 48°C to 57°C, and the storage temperature can be adjusted to prevent excessive outflow of the smoothing agent and agglomeration of the smoothing agent. Specifically, the storage temperature may be above 48°C, above 49°C, above 50°C, above 51°C, above 52°C, above 53°C, or above 54°C, and may be below 57°C, below 56°C, below 55°C, below 54°C, below 53°C, below 52°C, or below 51°C. If the storage temperature exceeds 57°C, the formability may be reduced, and if the storage temperature is less than 48°C, the smoothing agent will flow out excessively and agglomerate, which may cause a decrease in the reliability of the product due to process defects.
[0029] In one embodiment, the storage period during the above storage may be 10 to 300 days. Specifically, it may be more than 10 days, more than 20 days, more than 30 days, more than 40 days, more than 50 days, more than 60 days, more than 70 days, more than 80 days, more than 90 days, more than 100 days, more than 150 days, more than 200 days, or more than 250 days, and may be less than 300 days, less than 200 days, less than 100 days, less than 90 days, less than 80 days, less than 70 days, less than 60 days, less than 50 days, less than 40 days, less than 30 days, less than 20 days, or less than 10 days.
[0030] In one embodiment, the relative humidity during the above storage can be 5% to 25%. In the present disclosure, the "relative humidity (RH)" in this specification is a value expressing the ratio between the amount of water vapor currently contained in the air and the maximum saturated water vapor that can be contained in a specified volume of air in percentage (%).
[0031] In one embodiment, the surface roughness of the above-mentioned film is parameterized by the state in which the lubricant contained in the sealing layer of the above-mentioned film flows out to the above-mentioned sealing layer and the outer layer respectively and partially agglomerates. In the present disclosure, the roughness of the above-mentioned surface means the degree of fine concave-convex existing on the surface, that is, the surface roughness. Among the above-mentioned surface roughness parameters, Rt is the maximum height roughness, which is obtained by measuring the upper and lower distances between two parallel lines parallel to the center line and passing through the highest point and the lowest point of the curve in the roughness curve within the reference length (cut-off) of the intercepted portion. Rz is the ten point median height, which is obtained by measuring the distance between the average height from the highest peak to the fifth and the average valley depth from the lowest valley to the fifth.
[0032] In one embodiment, the black bag used in the measurement of the surface roughness is a bag having a matt black appearance and an outer layer formed of nylon (manufacturer: YOUL CHON Chemical Co., Ltd.). If the black bag is rubbed, the outer surface of the black bag and the sealing layer or outer layer of the film will produce friction, and the lubricant flowing out from the film will adhere to the surface of the black bag and form a white band. According to the present disclosure, when the film whose sealing layer contains a lubricant presents a surface roughness range, the lubricant flows out in small amounts and makes the size of the agglomerated particles very small, and it presents high formability. From the above viewpoint, when measured by the above method, the surface roughness value of the portion forming the white band can satisfy Rt 13μm to 20μm and Rz 10μm to 15μm. Among them, the surface roughness value can be the value when the sealing layer is rubbed once or the outer layer is repeatedly rubbed 5 times in the same direction. Specifically, the surface roughness Rt value (μm) may be 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, 18 or more, or 19 or more, 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, or 14 or less. Furthermore, the surface roughness Rz value (μm) may be 10 or more, 11 or more, 12 or more, 13 or more, or 14 or less, 15 or less, 14 or less, 13 or less, 12 or less, or 11 or less. Films having surface roughness Rt and Rz values outside the above ranges may have excessive lubricant outflow during lubricant inspection and may have aggregated particles of more than 60 μm on the surface of the sealing layer, and the friction coefficient and moldability of the sealing layer may be low.
[0033] From one point of view, the above-mentioned film of one embodiment can satisfy the following conditions: after being stored at a temperature of 48°C to 57°C for 30 days, when the outer surface of the black bag of the above-mentioned lubricant inspection device and the sealing layer or outer layer of the above-mentioned film are rubbed at a speed of 400mm / 10s using the same lubricant inspection device as described above, the average diameter of the largest agglomerated particles of the lubricant agglomerated particles existing in the portion where the lubricant flowing out of the above-mentioned film adheres to and forms a white band in the above-mentioned black bag is 60μm or less. The above-mentioned lubricant agglomerated particles mean particles formed by the agglomeration of the lubricant flowing out. The particle size is increased in such a way that the lubricant flows out excessively. The largest agglomerated particles of the above-mentioned lubricant agglomerated particles mean the largest agglomerated particles among the agglomerated particles formed, and the above-mentioned average diameter means the average value of the diameters measured in one agglomerated particle. Specifically, the largest agglomerated particle in the above-mentioned lubricant agglomerated particle size may mean the largest agglomerated particle in the total lubricant agglomerated particles reaching 100% or less, 98% or less, 96% or less, 94% or less, 92% or less, 90% or less, 88% or less, 86% or less, 84% or less, 82% or less, or 80% or less. Alternatively, specifically, the largest agglomerated particle in the above-mentioned lubricant agglomerated particle size may mean the largest agglomerated particle in the agglomerated particles contained in the image taken by a scanning electron microscope (SEM). Among them, the above-mentioned lubricant agglomerated particle size value may be the value when the sealing layer is rubbed once or the outer layer is repeatedly rubbed 5 times in the same direction. More specifically, the above-mentioned lubricant agglomerated particle size may be 60μm or less, 50μm or less, or 40μm or less. In one embodiment, the above-mentioned agglomerated particle size can be confirmed by a microscope image.
[0034] From one point of view, the film of one embodiment can reach a moldability of 15 mm to 25 mm after being stored at a temperature of 48° C. to 57° C. for 30 days. The moldability is determined by measuring the maximum depth that does not cause cracking when a pressure of 0.3 MPa is applied to the film and a cup (16 cm×9 cm) is molded. More specifically, the moldability can be 15 mm or more, 16 mm or more, 17 mm or more, 18 mm or more, 19 mm or more, 20 mm or more, 21 mm or more, 22 mm or more, or 23 mm or less, 25 mm or less, 24 mm or less, 23 mm or less, 22 mm or less, 21 mm or less, or 20 mm or less.
[0035] From one point of view, when the friction coefficient of the above-mentioned film of one embodiment is evaluated after being stored at a temperature of 48°C to 57°C for 30 days, the friction coefficient of the sealing layer of one embodiment disclosed can be 0.15 to 0.5: (a) After using the film of one embodiment of the present disclosure to manufacture a battery bag, prepare its test piece in a size of 200mm×100mm, and then bond it flatly to the bottom of the friction coefficient measuring device. (b) Thereafter, a test piece of 70mm×60mm size of the battery bag identical to the above-mentioned battery bag is fixed to a frame for measuring the friction coefficient. (c) Thereafter, after the frame set in the above-mentioned friction coefficient measuring device is attached between the two bags in a manner that the frame is in contact with the two above-mentioned bags, the bottom of the device is moved at a speed of 15mm / 1s for 55 seconds, thereby measuring the friction coefficient between the sealing layers of the two bags. In one embodiment, the above-mentioned friction coefficient measuring device can be a model CF-800XS of Labsink. Specifically, the friction coefficient may be greater than 0.15, greater than 0.2, greater than 0.25 or greater than 0.3, and may be less than 0.5, less than 0.4, less than 0.35, less than 0.3, less than 0.25 or less than 0.2.
[0036] In the present disclosure, as long as a battery pouch film can be manufactured, the material and thickness of each layer of the above film will not be limited, for example, the following structures may be included.
[0037] In the present disclosure, the sealing layer means a layer that is thermally bonded and given sealing properties after the battery is built in as an inner layer. As one embodiment, the sealing layer may include a hot adhesive resin, that is, a sealing resin for thermal bonding. Specifically, the sealing layer may include one or more selected from the group consisting of polyolefins such as polypropylene (PP), polyethylene (PE), and their copolymers, terpolymers or their derivatives, and ethylene vinyl acetate (EVA). As the above-mentioned copolymer (Co-polymer) or terpolymer (ter-polymer), ethylene / propylene copolymers or ethylene / propylene / butadiene terpolymers may be included. As one embodiment, the sealing layer may have a thickness of 20μm to 100μm. The sealing layer may be composed of multiple layers.
[0038] In the present disclosure, the slip agent means an additive for reducing the friction coefficient on the film surface and imparting lubricity and molding processing properties. In one embodiment, the slip agent may include one or more of waxes, amides, siloxanes, and silicon. Specifically, the slip agent may be an oleamide slip agent. More specifically, the slip agent may include one or more of erucamide, behenamide, stearamide, and oleamide.
[0039] In one embodiment, the film may include 0.1 weight percent to 20 weight percent of the lubricant relative to the total weight of the sealing layer. Specifically, relative to the total weight of the sealing layer, the film may contain a lubricant in an amount of 0.1 weight percent or more, 0.2 weight percent or more, 0.3 weight percent or more, 0.4 weight percent or more, 0.5 weight percent or more, 0.6 weight percent or more, 0.7 weight percent or more, 0.8 weight percent or more, 0.9 weight percent or more, 1 weight percent or more, 2 weight percent or more, 3 weight percent or more, 4 weight percent or more, 5 weight percent or more, 6 weight percent or more, 7 weight percent or more, 8 weight percent or more, 9 weight percent or more, 12 weight percent or more, 15 weight percent or more, 17 weight percent or more, or 19 weight percent or more, and may contain less than 20 weight percent, less than 17 weight percent, less than 15 weight percent, less than 13 weight percent, less than 10 weight percent, less than 9 weight percent, less than 8 weight percent, less than 7 weight percent, less than 6 weight percent, less than 5 weight percent, less than 4 weight percent, less than 3 weight percent, less than 2 weight percent, less than 15 weight percent, less than 13 weight percent, less than 10 weight percent, less than 9 weight percent, less than 8 weight percent, less than 7 weight percent, less than 6 weight percent, less than 5 weight percent, less than 4 weight percent, less than 3 weight percent, less than 2 weight percent, less than 1 weight percent, or less than 0.5 weight percent. If the lubricant is added in excess of the above range, the sealing strength may be reduced, the winding state may be poor, and the physical properties may become uneven over time, which may cause foreign matter problems in the process steps and hinder the reliability of the product. If the lubricant content is too low, the moldability may be deteriorated.
[0040] In the present disclosure, the outer layer means a layer having heat resistance, wear resistance, chemical resistance, etc. in order to protect the metal layer. As an embodiment, the outer layer may include one or more selected from the group consisting of polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polyhydroxy aldehyde (PHA), polylactic acid (PLA), thermoplastic starch (TPS), polyvinyl alcohol (PVA), polycaprolactam (PCL), polyethylene (PE), polypropylene (PP), ethylene vinyl acetate (EVA), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET) and nylon. More specifically, the outer layer may include one or more resins selected from the group consisting of nylon resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc. As an embodiment, the thickness of the outer layer may reach 5 μm to 40 μm. The outer layer may form a multi-layer structure.
[0041] In this specification, the metal layer means a barrier layer having the ability to block water vapor or air from outside the battery, gas and / or moisture generated inside the battery. As one embodiment, the metal layer may also include a surface treatment layer uniformly coated on one or both sides thereof. In one embodiment, the metal layer may be a metal film or a metal vapor-deposited layer. Examples of the metal film may include metal foil. The metal vapor-deposited layer may be formed by vacuum evaporating metal on a separate plastic film, for example, by vacuum evaporating metal on a film such as polyethylene terephthalate (PET), polyethylene (PE) or polypropylene (PP).
[0042] As an embodiment, as long as it has the barrier properties as described above, the metal of the above-mentioned metal layer is not limited in any way. For example, it can be one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), magnesium (Mg), nickel (Ni), tin (Sn), zinc (Zn), indium (In) and tungsten (W) (single metal or a mixture of single metals) or two or more alloys selected therefrom. Specifically, the above-mentioned metal may include one or more selected from the group consisting of aluminum or its alloys, titanium or its alloys, tungsten or its alloys, molybdenum or its alloys, copper or its alloys and stainless steel. More specifically, aluminum may be included. As an embodiment, in order to provide corrosion resistance to the metal, the above-mentioned surface treatment layer may be a surface treatment layer treated with phosphoric acid, chromium, zirconium, cerium, lanthanum, scandium, yttrium, etc.
[0043] As an embodiment, the thickness of the metal layer can be 20 μm to 80 μm. If the thickness of the metal layer is less than 20 μm, pin holes, fine gaps, etc. may be generated during the molding process, making it difficult to ensure safety. If the thickness of the metal layer is greater than 80 μm, the energy density may decrease during battery manufacturing.
[0044] In one embodiment of the present disclosure, an adhesive layer for bonding the metal layer to the outer layer may be included between the metal layer and the outer layer. And, in one embodiment of the present disclosure, an adhesive layer for bonding the metal layer to the sealing layer may be included between the sealing layer and the metal layer. Specifically, the adhesive layer may be an adhesive layer and / or an extruded resin layer. For example, the adhesive layer may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenol resin adhesive, a polyolefin adhesive, and a polyester adhesive. As one embodiment, the thickness of the adhesive layer may reach 0.5μm to 10μm. For example, the extruded resin layer may include an olefin resin such as a polypropylene resin. As one embodiment, the thickness of the extruded resin layer may reach about 5μm to 80μm.
[0045] An embodiment of the present disclosure may provide a battery pouch including the film for a battery pouch as described above.
[0046] Another embodiment of the present disclosure may provide a method for preserving the above-mentioned battery bag film, which includes the step of preserving at a temperature of 48°C to 57°C. Specifically, the above-mentioned storage temperature may be above 48°C, above 49°C, above 50°C, above 51°C, above 52°C, above 53°C, or above 54°C, and may be below 57°C, below 56°C, below 55°C, below 54°C, below 53°C, below 52°C, or below 51°C. If the storage temperature exceeds 57°C, it may lead to a decrease in formability. If the storage temperature is less than 48°C, the lubricant will flow out too much and cause poor process, thereby reducing product reliability.
[0047] In one embodiment, the storage period of the above-mentioned storage step may be more than 10 days. Specifically, it may be more than 10 days, more than 20 days, more than 30 days, more than 40 days, more than 50 days, more than 60 days, more than 70 days, more than 80 days, more than 90 days, more than 100 days, more than 150 days, more than 200 days, or more than 250 days, and may be less than 300 days, less than 200 days, less than 100 days, less than 90 days, less than 80 days, less than 70 days, less than 60 days, less than 50 days, less than 40 days, less than 30 days, or less than 20 days.
[0048] In one embodiment, the relative humidity in the storage step can reach 5% to 25%.
[0049] Hereinafter, the present disclosure will be described in more detail by way of examples. These examples are only used to illustrate the present disclosure, and the scope of the present disclosure is not limited to these examples, which is self-evident to those skilled in the art.
[0050] [Manufacturing example]
[0051] An embodiment of the present disclosure is manufactured by the following method.
[0052] A 25 μm outer layer is formed of a polyethylene terephthalate film on one side of a 60 μm thick metal layer made of an aluminum foil metal raw material, and an 80 μm sealing layer is formed by bonding an unstretched polypropylene film containing an amide lubricant in an amount of 0.1 to 20 weight percent relative to the total weight of the sealing layer to the other side of the metal layer, thereby manufacturing a battery bag film.
[0053] As one embodiment of the present disclosure, the outer layer may be a laminate of a 12 μm polyethylene terephthalate film and a 25 μm nylon film to produce a battery bag film. In this case, the results of the test example obtained were confirmed to be the same as those of the test examples described below.
[0054] [Test Example 1]
[0055] The following experiment was conducted to confirm the surface roughness of the film produced in the above-mentioned production example at the time of storage at the storage temperature.
[0056] First, a lubricant inspection device was prepared in the form of a black bag (manufacturer: YOUL CHON Chemical) wrapped around the surface of a regular hexahedron-shaped metal (iron, weight: about 1.3 kg). The film produced in the above manufacturing example cut into a size of 50 mm × 240 mm was fixed on a flat surface so that the sealing layer was located on the top, and then the black bag of the above device was rubbed once at a speed of 400 mm / 10 s on the sealing layer of each film stored at different storage temperatures.2 The portion where the lubricant flowing out of the above-mentioned film adheres to form a white band on the above-mentioned black bag is cut to a size of , and after being flatly attached to a slide glass using a double-sided tape, the surface roughness is measured using a surface roughness measuring device (for example, NV-2200 3D profiler, a product of Nano system, Inc.) and an analysis program (NanoMap, a product of Nano system, Inc.).
[0057] Among them, Figure 1 And Table 1 shows the results of Example 1 and Example 2 and Comparative Example 4.
[0058]
Table 1
[0059]
[0060] As shown in the above results, it was confirmed that in Examples 1 and 2 of the present disclosure, the surface roughness was adjusted to be within the ranges of Rt 13 μm to 20 μm and Rz 10 μm to 15 μm by adjusting the storage temperature.
[0061] [Test Example 2]
[0062] In order to confirm the improvement of lubricant aggregation, friction coefficient and formability based on the surface roughness of the film of one embodiment of the present disclosure, the following experiments were carried out on Example 1, Example 2 and Comparative Examples 1 to Comparative Examples 4, which confirmed the surface roughness in the above-mentioned Test Example 1, and the respective measured values are shown in Tables 2 to 9. In this case, on day 0, the formability, lubricant test and friction coefficient of each film were measured at room temperature, and then the results were observed for 90 days by storing at various set storage temperatures.
[0063] Lubricant inspection
[0064] The lubricant inspection is used to measure the amount or aggregation pattern of the lubricant flowing out to the sealing layer or outer layer surface of the battery bag film. The same lubricant inspection device as used for measuring the above-mentioned surface roughness is prepared. After cutting the above-mentioned film into a size of 50mm×240mm, it is fixed on a flat surface in a manner that the sealing layer or outer layer is located on the top, and then the sealing layer or outer layer of the prepared above-mentioned film is rubbed at a speed of 400mm / 10s for friction. In the case of rubbing the sealing layer, rubbing is performed once, and in the case of rubbing the outer layer, it is repeated 5 times. Afterwards, a scanning electron microscope (SEM. Manufacturer: HITACHI, Product Name: SU3500) is used to photograph the part where the lubricant flowing out of each of the above-mentioned films adheres to and forms a white band on the above-mentioned black bag, and the size of the lubricant aggregation particles is confirmed and evaluated with the naked eye. Figure 2To take a photo of the lubricant inspection device used in the above experiment, Figure 3 After the above experiment, an image of a black bag was taken, and a white band was confirmed to be formed on the upper part of the black bag image. Figure 4 As shown in the figure, the results of visual evaluation are as follows: if only one side of the corner is seen and there are few scratches on most of the area, it is evaluated as S grade; if two stripes appear in the corner (white band area) and there are scratches of the lubricant, it is evaluated as A grade (A+, A0 or A-); if two stripes appear in the corner and the lubricant is adhered to all surfaces, it is evaluated as B grade.
[0065] Furthermore, when SEM image analysis was performed, the number of the largest aggregated particles selected from the aggregated particles of the lubricant present in the portion where the lubricant was applied to form a white band on the black bag and the average diameter thereof were confirmed.
[0066] Determination of friction coefficient
[0067] After the prepared films were cut into 200mm×100mm sizes, the friction coefficients of the films were measured using a friction coefficient measuring instrument (manufacturer: Labsink, product name: CF-800XS). Specifically, after preparing a test piece of the film in a size of 200mm×100mm, it was flatly bonded to the bottom of the friction coefficient measuring device, and then a test piece of the same film in a size of 70mm×60mm was attached to the required frame of the friction coefficient and connected to the equipment with a rope. After placing the two films in contact with each other, the bottom of the equipment was moved at a speed of 15mm / 1s for 55 seconds, and the film of the frame fixed with a rope was fixed, thereby measuring the friction coefficient between the two films.
[0068] Determination of formability
[0069] After the prepared film was cut into 200 mm × 100 mm sizes, a pressure of 0.3 MPa was applied to a cup-shaped molding frame (manufacturer: GWANGSHIN Hi-Tech, model: GS-S5) to mold the film, and the maximum depth at which no cracks or ruptures occurred during molding was measured. In this case, among the same 10 film test pieces, if all 10 test pieces were not broken, a deeper depth was used, and if one was broken, the previous depth was defined as the maximum height.
[0070]
Table 2
[0071] Comparative Example 1
[0072]
[0073]
Table 3
[0074] Comparative Example 2
[0075]
[0076]
[0077] [Table 4] Comparative Example 3
[0078]
[0079] [Table 5] Comparative Example 4
[0080]
[0081]
Table 6
[0082] Example 1
[0083]
[0084]
Table 7
[0085] Example 2
[0086]
[0087] [Table 8] Comparative Example 5
[0088]
[0089]
[0090] Figure 5A , Figure 5B , Fig. 6A as well as Figure 6B The following is a result of analyzing the size of particles formed by agglomerating the lubricant that flowed out after the above lubricant inspection. Figure 5A as well as Figure 5B The average diameter of the largest aggregated particles present in the SEM image of the film of Example 1 in the above table was 39.2 μm. Fig. 6A as well as Figure 6B These are images of the film of Comparative Example 4 in the above table. The average diameter of the largest aggregated particles in the SEM image of Comparative Example 4 is 40.9 μm, and the average diameter of the largest aggregated particles in the SEM image of Comparative Example 4 is 97.5 μm.
[0091] The above results are summarized and shown in the following table.
[0092]
Table 9
[0093]
[0094] As shown in the above results, unlike Comparative Examples 1 to 4, Examples 1 and 2 of the present disclosure satisfy the range of surface roughness Rt 13μm to 20μm and Rz 10μm to 15μm, and the size of the lubricant agglomerated particles present on the surface of the sealing layer is reduced to less than 60μm when the lubricant is inspected. In addition, in Examples 1 and 2, the friction coefficient of the silane layer is maintained at more than 0.15, and the moldability is increased by about 40% compared to that at room temperature (day 0), showing high moldability while a small amount of lubricant flows out.
[0095] [Test Example 3]
[0096] Films were manufactured according to the above manufacturing examples, and by adjusting their storage temperatures, Examples 3 and 4 satisfying the surface roughness ranges of Rt 13 μm to 20 μm and Rz 10 μm to 15 μm of the films, and Comparative Examples 5 to 8 exceeding the above ranges were prepared. In order to confirm the lubricant aggregation pattern, friction coefficient and formability based on the surface roughness of the above films, the surface roughness, lubricant inspection, friction coefficient and formability of each film were measured in the same manner as described in the above Test Examples 1 and 2, and the respective measured values are shown in Table 10.
[0097]
Table 10
[0098]
[0099] As a result, Examples 3 and 4 of the present disclosure, which satisfy the ranges of surface roughness Rt 13 to 20 and Rz 10 to 15, both obtained S grade in the lubricant test results, showing a high friction coefficient of 0.2 or more. In addition, although Examples 3 and 4 contain the same amount of lubricant as Comparative Examples 5 to 8, the outflow amount of the lubricant is adjusted so as to satisfy the above surface roughness values, and it can be confirmed that the moldability is significantly improved.
[0100] As an embodiment, the present disclosure may provide the following implementation methods.
[0101] [First embodiment]
[0102] A film for a battery bag comprises: a sealing layer containing a lubricant; a metal layer formed on the sealing layer; and an outer layer formed on the metal layer, wherein after the film is stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black bag with a matt black appearance and an outer layer made of nylon is used to rub the outer surface of the black bag and the sealing layer or outer layer of the film at a speed of 400mm / 10s, the surface roughness value of the portion to which the lubricant flowing out of the film adheres and forms a white band on the black bag satisfies Rt 13μm to 20μm and Rz 10μm to 15μm.
[0103] [Second embodiment]
[0104] According to the battery bag film described in the first embodiment, after the above-mentioned film is stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black bag with a matt black appearance and an outer layer made of nylon is used to rub the outer surface of the above-mentioned black bag and the sealing layer or the outer layer of the above-mentioned film at a speed of 400mm / 10s, the average diameter of the largest agglomerated particles of the lubricant flowing out of the above-mentioned film that adheres to the part of the above-mentioned black bag to form a white band is less than 60μm.
[0105] [Third Embodiment]
[0106] According to the battery pouch film of the first embodiment or the second embodiment, after the film is stored at a temperature of 48° C. to 57° C. for 30 days, the friction coefficient of the sealant layer is 0.15 to 0.5.
[0107] [Fourth Embodiment]
[0108] According to any one of the first to third embodiments, the battery bag film has a moldability of 15 mm to 25 mm after being stored at a temperature of 48° C. to 57° C. for 30 days, wherein the moldability is a maximum depth that does not cause rupture when a pressure of 0.3 MPa is applied to the film to form a cup.
[0109] [Fifth Embodiment]
[0110] According to any one of the first to fourth embodiments, the film is stored at a temperature of 48°C to 57°C.
[0111] [Sixth Embodiment]
[0112] According to any one of the first to fifth embodiments, the film comprises 0.1 to 20 weight percent of a smoothing agent relative to the total weight of the sealing layer.
[0113] [Seventh Embodiment]
[0114] According to any one of the first to sixth embodiments, the lubricant includes at least one of waxes, amides, siloxanes, and silicon.
[0115] [Eighth Embodiment]
[0116] According to any one of the first to seventh embodiments, the metal layer includes one or more selected from the group consisting of aluminum or its alloy, titanium or its alloy, tungsten or its alloy, molybdenum or its alloy, copper or its alloy, and stainless steel.
[0117] [Ninth Embodiment]
[0118] According to any one of the first to eighth embodiments, the outer layer includes one or more selected from the group consisting of polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polyhydroxy aldehyde (PHA), polylactic acid (PLA), thermoplastic starch (TPS), polyvinylalcohol (PVA), polycaprolactam (PCL), polyethylene (PE), polypropylene (PP), ethylene vinyl acetate (EVA), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET) and nylon.
[0119] [Tenth embodiment]
[0120] According to the battery pouch film of any one of the first to ninth embodiments, the sealant layer contains a thermal adhesive resin.
[0121] [Eleventh Embodiment]
[0122] A storage method for storing the battery pouch film according to any one of the first to tenth embodiments, comprising the step of storing the film at a temperature of 48° C. to 57° C.
[0123] [Twelfth Embodiment]
[0124] According to the storage method described in the eleventh embodiment, the storage period of the above steps is 10 days to 300 days.
[0125] [Thirteenth Embodiment]
[0126] According to the storage method of the eleventh or twelfth embodiment, when the storage is performed in the above step, the relative humidity is 5% to 25%.
Claims
1. A battery bag film, characterized in that: include: a sealing layer, including a lubricant; a metal layer formed on the sealing layer; and An outer layer, formed on the above metal layer, After the above-mentioned film is stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black bag with a matte black appearance and an outer layer made of nylon is used to rub the outer surface of the above-mentioned black bag and the sealing layer or outer layer of the above-mentioned film at a speed of 400mm / 10s, the surface roughness value of the part where the lubricant flowing out of the above-mentioned film adheres to and forms a white band on the above-mentioned black bag satisfies Rt 13μm to 20μm and Rz 10μm to 15μm.
2. The battery bag film according to claim 1, characterized in that: After the above-mentioned film was stored at a temperature of 48°C to 57°C for 30 days, when a lubricant inspection device in the form of a 1.3kgf regular hexahedral metal wrapped in a black bag with a matte black appearance and an outer layer made of nylon was used to rub the outer surface of the above-mentioned black bag and the sealing layer or outer layer of the above-mentioned film at a speed of 400mm / 10s, the average diameter of the largest agglomerated particles of the lubricant flowing out of the above-mentioned film that adhered to the part of the above-mentioned black bag to form a white band was less than 60μm.
3. The battery bag film according to claim 1, characterized in that: After the film was stored at a temperature of 48° C. to 57° C. for 30 days, the friction coefficient of the sealing layer was 0.15 to 0.
5.
4. The battery bag film according to claim 1, characterized in that: After the above film was stored at a temperature of 48°C to 57°C for 30 days, the moldability was 15 mm to 25 mm. The moldability is the maximum depth at which cracks do not occur when the film is molded into a cup under a pressure of 0.3 MPa.
5. The battery bag film according to claim 1, characterized in that: The membranes were stored at a temperature of 48°C to 57°C.
6. The battery bag film according to claim 1, characterized in that: The film comprises 0.1 to 20 weight percent of the lubricant relative to the total weight of the sealing layer.
7. The battery bag film according to claim 1, characterized in that: The lubricant includes at least one of waxes, amides, siloxanes and silicon.
8. The battery bag film according to claim 1, characterized in that: The metal layer includes at least one selected from the group consisting of aluminum or its alloy, titanium or its alloy, tungsten or its alloy, molybdenum or its alloy, copper or its alloy, and stainless steel.
9. The battery bag film according to claim 1, characterized in that: The outer layer includes one or more selected from the group consisting of polybutylene adipate terephthalate, polybutylene succinate, polyhydroxy aldehyde, polylactic acid, thermoplastic starch, polyvinyl alcohol, polycaprolactam, polyethylene, polypropylene, ethylene vinyl acetate, ethylene-vinyl alcohol, polyvinylidene chloride, polyethylene terephthalate and nylon.
10. The battery bag film according to claim 1, characterized in that: The sealing layer contains a thermal adhesive resin.
11. A storage method for storing the battery pouch film according to any one of claims 1 to 10, characterized in that: The method comprises the step of storing the film at a temperature of 48°C to 57°C.
12. The storage method according to claim 11, characterized in that: The shelf life of the above steps is 10 to 300 days.
13. The storage method according to claim 11, characterized in that: When storing in the above steps, the relative humidity is 5% to 25%.
Citation Information
Patent Citations
Packaging material for power storage device, packaging case for power storage device, and power storage device
CN108023032A
Polypropylene-based composite film, laminate using same, packaging pouch for battery exterior, and retort packaging pouch
CN109952202A
Sealant film
CN113874210A
A anode active material for a lithium ion battery, a method for manufacturing the same, a anode for a lithium ion battery comprising the anode active material and a lithium ion battery comprising the anode
KR1020210158025A