Composite glass, in particular for vehicle

By combining a porous glaze coating with an uncolored polymer layer in the composite glass, the problems of coating delamination and uneven color tone are solved, improving the mechanical strength and appearance stability of the composite glass and ensuring driving safety.

CN119017793APending Publication Date: 2024-11-26SCHOTT AG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410639316.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The coating of existing composite glass is prone to delamination during the thermoforming process, which affects its strength and appearance stability. In addition, the existing porous coating has poor compatibility with the polymer layer, resulting in uneven color of the composite and affecting driving safety.

Method used

A porous glaze coating is combined with an uncolored polymer layer. The coating contains a glass plate with SiO2 and B2O3, and contains pigments and additives. The polymer layer partially fills the pores of the coating to form a continuous porous structure, ensuring good bonding between the coating and the polymer layer.

Benefits of technology

This technology improves the mechanical strength and appearance stability of composite glass, avoids coating delamination, provides a uniform dark appearance, simplifies the manufacturing process, and enhances driving safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017793A_ABST
    Figure CN119017793A_ABST
Patent Text Reader

Abstract

The present invention generally relates to a composite glass, in particular for a vehicle. The invention relates in particular to a composite glass, for example for vehicles, which is suitable for use as a windshield, for example, and which has particularly good strength and very good user safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a composite glass, in particular for vehicles. In particular, the present invention relates to a composite glass, for example for vehicles, which is suitable, for example, for use as a windshield and has particularly good strength and very good user safety. Background Art

[0002] Composite glazing is, for example, the choice for automotive glazing, in particular in particularly critical areas such as windshields. Composite glazing generally comprises at least two glass panes which are bonded together by a polymer layer arranged between the panes. If a glass pane breaks due to mechanical action, the polymer layer, which can be in the form of a film, for example, holds the glass pane fragments together, thereby minimizing damage to vehicle occupants due to glass breakage.

[0003] Such window panes are exposed to abrasive conditions, i.e. abrasion due to particles that hit the window pane at high speeds (e.g. also known as "rockfall"), and therefore it is advantageous to use a composite material having the composition SiO 2 and B 2 O 3 A plate of glass of WO2008006004 is used as the outer glass plate of the plate composite. In the context of the present disclosure, such glass is also generally referred to as borosilicate glass. It is well known that such glass has good scratch resistance and many other advantages, such as generally good mechanical stability and heat resistance.

[0004] It is known that, for example, a product named Commercially available borosilicate glasses are used for the outer glazing of vehicle windows. These glasses are very suitable, for example, for laminated glazings and are distinguished by very high transmittance in the visible light range. In addition, borosilicate glasses generally have very good heat resistance, high chemical resistance and good mechanical strength.

[0005] For example, international patent application WO 2015 / 059406 A describes a laminated glass pane. One of the panes (eg the outer pane) may, for example, comprise borosilicate glass.

[0006] International patent application WO 2017 / 157660A1 describes a composite glass pane for a head-up display. Here, one of the panes of the composite glass can also include borosilicate glass.

[0007] CO 2017 / 005596 A1 also describes an automotive glass pane with increased durability.

[0008] International patent application WO 2019 / 130285 A1 describes a laminate with high durability against wear and environmental influences.

[0009] Finally, international patent application WO 2018 / 122769A1 describes a laminate having a higher breaking strength.

[0010] As mentioned above, the windshield is designed as a composite glass sheet to ensure the safety of vehicle passengers. Moreover, the windshield usually also has a coating in the edge area. On the one hand, the coating is used to optically shield, for example, adhesives or components (such as antennas), and on the other hand, the coating is also used to protect, for example, adhesives or components (such as antennas) from ultraviolet radiation. Generally speaking, the coating is arranged between two glass sheets of the composite, wherein the coating can therefore be arranged in the form of a frame, for example. In addition, as also mentioned above, the composite also includes a polymer layer (i.e., a layer containing a polymer or a layer composed of a polymer) arranged between the two glass sheets, which connects the glass sheets to each other. Usually, the glass sheets with the coating arranged therebetween in at least one area, especially in the edge area, are stacked on each other and bent during the hot forming process. However, in general, and not limited to the examples described herein, the glass sheets of the composite can also be formed individually and independently of each other. Then the polymer layer is introduced between the two sheets and the bent glass sheets are combined together, so that a composite glass sheet is finally obtained. In the case of the present disclosure, such a composite glass sheet is also referred to as "composite glass (Verbundglas)". For such composite glasses, the terms “glass composite” or “composite” can also be used synonymously.

[0011] Therefore, many requirements are placed on the glass panes that are included in such composites. Since the bending process takes place under hot conditions, the glass panes and the coatings applied to them must be able to withstand these temperatures. The glass panes and the coating must be able to bond with the polymer layer so that a stable composite is formed and no delamination between glass and polymer occurs. Finally, the coating needs to be sufficiently optically impermeable so that components arranged in the frame area of ​​the windshield are not obtrusively visible. This prevents the driver of the vehicle from being distracted and thus increases driving safety. Microcracks or other defects in the coating should also be avoided or at least minimized as far as possible.

[0012] In addition to the heat resistance of the glass and the coating, the above-mentioned compatibility of the glass or the coating with the polymer material to form a composite, the optical density and the minimization of possible defects and in general the mechanical strength of the individual glass panes, in particular the coated glass panes, it is also particularly important that the coating is preferably homogeneous, preferably black or dark in color. It is generally known that coatings on glass panes, including composite glass panes, can affect the strength of the glass panes and ultimately also the strength of the resulting composite glass, especially if the adhesion strength of these coatings is particularly high. In addition, there is the following difficulty: on the one hand, layers with particularly high adhesion strength are required in order to prevent delamination of the layers, while on the other hand, these layers with relatively high adhesion strength actually reduce the strength of the glass.

[0013] In order to give the glass sheets and the resulting composites good mechanical stability, such layers can, for example, be formed in a porous manner or have a sol-gel adhesive instead of a glass-based adhesive. It is almost certain that the strength reduction caused by one or more layers is partly based on the formation of so-called "melt reaction zones", which are caused by the use of conventional glass-based coatings. On the other hand, however, if the thermal expansion of the layer and the substrate is significantly different, even the formation of a very dense layer can lead to a reduction in strength. This can be reduced, for example, by forming the coating in a porous manner. This can be achieved, for example, by using a sol-gel adhesive, in which case no so-called melt reaction zones are formed, which is also advantageous with regard to strength.

[0014] However, the disadvantage of forming the coating in a porous manner and / or using a sol-gel binder is that it has not been possible to produce particularly good glass composites in this way so far. This is because, as mentioned above, the glass composite is produced by laminating at least two sheets of the composite by means of a polymer layer. Depending on the composition of the sol-gel binder, the compatibility with the polymer may be reduced, so that a stable composite cannot be formed, especially in the region of the coating. In addition, porous coatings may have insufficient adhesion or may result in a very unstable, spotty appearance of the coating, which is of great importance for driver safety, since the unstable appearance may distract the driver.

[0015] Therefore, there is a need for composite glasses that at least alleviate the above-mentioned disadvantages of the prior art. Summary of the invention

[0016] The object of the present invention is to provide a composite glass which at least partially alleviates the above-mentioned disadvantages of the prior art.

[0017] The solution of the invention for achieving the above mentioned objects lies in the subject matter of the independent claims. Advantageous, preferred and specific embodiments refer to the dependent claims, the description and the drawings of the present disclosure.

[0018] The present invention therefore generally relates to a composite glazing, in particular for vehicles, comprising two glass panes, at least one of which is partially coated and comprises a SiO-containing composite glazing. 2 and B 2 O 3 A glass sheet of glass having a first side and a second side.

[0019] At least one coating is applied in at least one region of the second side of the at least one glass pane.

[0020] The at least one coating is formed as an enamel coating, which comprises at least one pigment, a glass component and preferably at least one additive. The additive can be in the form of a filler, in particular.

[0021] The at least one coating comprises pores, preferably open pores, so that in the at least one coating, a direct connection is preferably produced between the side of the at least one coating facing the second side of the at least one glass pane and the side of the at least one coating facing away from the second side of the at least one glass pane.

[0022] Preferably, the at least one glass sheet has a flexural strength of at least 5 MPa to at most 170 MPa, preferably at least 20 MPa to at most 170 MPa, more preferably at least 35 MPa, particularly preferably at least 60 MPa, most preferably at least 80 MPa.

[0023] Furthermore, the composite glass comprises at least one polymer layer arranged between the glass panes, wherein the polymer of the polymer layer is present in an uncolored manner and wherein in the region of the at least one coating at least a portion of the polymer layer at least partially fills pores of the at least one coating.

[0024] This results in color coordinates of the composite glass in the CIEL*a*b* system, which are measured in the viewing direction from the first side to the second side of the at least one glass pane in at least one region where the first coating is applied to the second side of the at least one glass pane, wherein L* is at most 12 and preferably at least 1, and a* and b* are in the range between +5 and -5. In other words, the color coordinates are measured or determined through the glass pane.

[0025] In the context of this disclosure, the following definitions apply:

[0026] Composite glass generally refers to a composite body comprising at least two glass sheets, which are firmly bonded to each other via an intermediate layer. Composite glass may also be generally referred to as a "composite body", "sheet composite body", "glass composite body", "composite glass sheet" or the like.

[0027] A plate generally refers to a formed body whose lateral dimension in a first spatial direction of a Cartesian coordinate system is at least one order of magnitude smaller than the lateral dimensions in the other two spatial directions perpendicular to the first spatial direction. This lateral dimension along the first spatial direction may also generally be referred to as the "thickness" of the plate, and the other two lateral dimensions are referred to as "length" and "width". In other words, according to the present disclosure, the thickness of the plate is at least one order of magnitude smaller than its length and width. Within the scope of the present disclosure, the length and width of the plate may be of the same order of magnitude, or the length of the plate may be significantly greater than the width. Therefore, a plate in the sense of the present disclosure also includes a design as a strip.

[0028] A glass pane is generally understood to mean that the pane comprises glass, for example consists of glass. A glass pane can generally be coated, ie formed as a coated glass pane.

[0029] In the context of the present disclosure, the sides of a glass sheet are referred to as the main sides or main surfaces. As mentioned above, a sheet is a shaped body whose thickness is significantly less than the length and width. The length and width of such a plate-like shaped body (or sheet) define the main sides, which together occupy more than 50% of the total surface area, usually much more than this, especially in the case of very thin sheets. Therefore, these main sides or sides are opposite to the peripheral edge faces of the sheet. Therefore, in the sense of the present disclosure, a sheet generally comprises two sides, which may also be referred to as top and bottom sides or front and back sides, as the case may be.

[0030] In the context of the present disclosure, the terms "layer" and "coating" are to be understood synonymously as follows: a layer is a material layer which is applied to a substrate having a material composition which differs greatly from that of the coating or layer by means of a special process (so-called coating process). In the context of the present disclosure, such coating processes may in particular be coating processes such as printing (preferably screen printing or pad printing), coating rolls, application as a film or brushing, but dipping and spraying or other further coating processes may also be used in general. The coating or material layer may also generally be applied in laminated form, for example by laminating films. Therefore, within the scope of the present disclosure, a polymer layer of a composite may generally be understood as a material layer in the sense of the present disclosure.

[0031] In the context of the present disclosure, an enamel coating is generally understood to mean a coating comprising at least one glassy component which is adhered to the substrate by a thermal process. In addition to the glassy component, the enamel coating may also contain further components, in particular at least one pigment and possibly one or more additives, such as one or more fillers or so-called foaming agents. In the present case, the glassy component is understood to mean an inorganic and amorphous component, in particular comprising SiO 2 . The glassy component can in particular be produced by a melting process or consist of glass. Glass generally refers to an inorganic, amorphous solid obtained by a melting process. The glass is generally a silicate glass. The glassy component in the glaze coating can in particular be formed as a glass flow (Glasfluss) or glass powder (Glasfritte). These terms are well known to those skilled in the art in the field of glass coating. In the case of the present disclosure, the glaze coating can be formed so that the glassy component is completely melted, flows onto the underlying substrate (here in particular a glass plate), and covers the other components of the coating (such as pigment particles), but the glaze coating can also be formed as a sintered coating, which means that the glassy component is only partially melted in a thermal process (which can also be referred to as firing). This may be preferred, in particular when it is necessary to achieve a coating containing pores.

[0032] In the context of the present disclosure, pigment refers to a color body, i.e. a solid with an intrinsic color. It is usually present in the form of particles. That is, in the context of the present disclosure, if a coating contains a pigment, it means that the coating contains solid particles with a specific composition. This also applies to so-called fillers accordingly. In this case, fillers are solids that are added to a coating or layer in the form of particles to affect a certain property of the coating, wherein these fillers are not primarily related to the color of the coating, but to other properties such as thermal expansion, scratch resistance, etc.

[0033] A polymer layer refers to a material layer containing a polymer or consisting of a polymer. The polymer layer can be in particular in the form of a polymer film. A polymer is an organic macromolecule. In the context of the present disclosure, when referring to a layer or film "consisting of" a certain polymer, it means that the layer includes the polymer as an essential component, but, as is generally common in the plastics industry, may also have other components, which can be referred to as so-called additives.

[0034] The “uncolored” design of a material or a material layer means that it is colorless in the visible light range, i.e., in the range from 380 nm to 780 nm, i.e., has neutral color coordinates and preferably has a high transparency in this wavelength range. The transmittance (τ vis) is preferably at least 70% in order to meet the requirements for using the glass sheet composite as a windshield, for example. The minimum transmittance of a windshield is usually greater than 70%. If glare occurs at less than 0.1 m 2 If the area of ​​the upper auxiliary viewing area is larger than 0%, it is allowed to use an anti-glare wedge in the upper auxiliary viewing area to block the glare. Such an area for blocking (i.e., down to a 0% transmittance gradient) can be formed at the edge of the plate. In Europe, the standard for this is ECE R43 (Regulation 43 of the United Nations Economic Commission for Europe (UNECE) - Uniform provisions concerning the approval of safety glazing materials and their installation in vehicles - Official Journal of the European Union L42 / 1; November 3, 2013).

[0035] A layer or coating containing pores is understood to be a coating formed in a porous manner. This is to be understood in particular as a coating having open porosity, preferably even continuous pores. Continuous pores or continuous porosity means the presence of fluid channels which connect a first side of a material layer with a second side of the material layer opposite the first side.

[0036] The above-described embodiments of the composite glass have many advantages, which will be described below by way of examples.

[0037] The composite glass comprises at least two glass sheets, wherein at least one glass sheet comprises SiO 2 and B 2 O 3 Glass panes made of glass of a preferred embodiment of the present invention are borosilicate glass panes. As described above, such glass panes have good mechanical strength (in particular breaking strength), high heat resistance and good scratch resistance (which can also be understood as resistance to attack by small sharp objects or something similar in general). For example, such glasses also have very good chemical resistance, compared to soda-lime glass. This is particularly important for vehicle windows, which can be exposed to salt mist, for example in winter, which can also cause so-called glass corrosion. In this regard, the higher chemical resistance of borosilicate glass compared to the known soda-lime glass can be advantageous.

[0038] At least one coating is arranged in at least one region of at least one pane consisting of borosilicate glass or containing borosilicate glass. This generally means that the composite glass comprises at least one coating, wherein in particular it can also be provided that the composite glass comprises only a single coating. However, the composite glass can also comprise further coatings. These coatings can be arranged in the region having the at least one coating or can partially overlap with the coating; however, this is not absolutely necessary.

[0039] The at least one coating is a coating intended to form a preferably light-impermeable area, preferably in the edge area of ​​at least one glass pane or in a manner corresponding to composite glazing, for example as a lamination of pipelines, etc., but also partly as sun or glare protection for vehicle occupants, for example the vehicle driver. According to one embodiment, the at least one coating can be in the form of a frame, i.e. in the form of an area around the edge of one side of the glass pane.

[0040] For this purpose, the at least one coating is designed as a dyed coating, i.e. a colored coating. The at least one pigment contained in the at least one coating ensures that the coating has a sufficient optical density so that the electronic components are not obtrusively visible and / or that the coating can achieve its purpose as a light shielding / anti-glare protection. The at least one coating is designed as an enamel coating which, as described above, comprises at least one pigment and a vitreous component. Such enamel coatings, due to their vitreous structure, not only have good chemical resistance and mechanical stability, but are also well compatible with a vitreous substrate, such as the glass panes described here, so that relatively good adhesion strengths can generally also be achieved thereby.

[0041] Preferably, the glass pane can be formed (in particular by forming the at least one coating itself) such that its bending strength is between at least 5 MPa and at most 170 MPa, preferably between at least 20 MPa and at most 170 MPa, more preferably at least 35 MPa, particularly preferably at least 60 MPa, most preferably at least 80 MPa. Therefore, the coating and / or the at least one glass pane are preferably formed such that the inherent strength of the glass pane is maintained or only slightly reduced.

[0042] As mentioned above, the composite glazing comprises a polymer layer arranged between the glass sheets, wherein the polymer of the polymer layer is not colored. In other words, the polymer of the polymer layer and therefore the entire polymer layer is transparent. Of course, this is not only advantageous but also absolutely necessary in the visible area of ​​the vehicle window. However, it is known in the composite glazing known in the prior art that the polymer layer can also be colored in the area of ​​at least one coating. In the case of the composite glazing of the prior art, for example, a polymer layer that imitates the frame and is colored itself can be arranged in the frame area, for example in the area of ​​at least one coating. In this case, for obvious reasons, an uncolored polymer layer is therefore arranged in the visible area. Therefore, in the prior art, in order to enable the composite glazing to have sufficient transparency in the visible area, but at the same time to produce sufficient opacity in the edge area, two different polymer layers, such as two different polymer films, are sometimes required.

[0043] According to the present disclosure, it is not necessary but preferred to form an uncolored polymer layer between the sheets of composite glass. In particular, in the region of at least one coating, the polymer layer is preferably also uncolored. The polymer layer can, for example, be arranged over the entire surface between two glass sheets.

[0044] Of course, for other reasons, such as to achieve better adhesion of a particular polymer on the coating, a “dual film” or “dual polymer” solution may also be employed according to the present disclosure.

[0045] Nevertheless, with the composite glazing according to the disclosure, even when using only a single polymer layer arranged over the entire surface between the glass panes, a uniform dark color coordinate of the composite glazing can be achieved, which color coordinate is measured in the viewing direction from the first side to the second side of the at least one glass pane in at least one region in which the at least one coating is arranged. This is possible because the at least one coating is formed in a porous manner, preferably with a continuous open porosity, and therefore in the region of the at least one coating at least a portion of the polymer layer at least partially fills the pores of the at least one coating.

[0046] The porous design of the at least one coating means that the coating does not significantly affect the mechanical strength of the at least one glass pane, for example only slightly reduces it. However, this also results in the coating or the corresponding glass composite being less neutral in color and darker in color. This is because the pores cause scattering and thus an unstable appearance, which means that the component is not sufficiently concealed and the vehicle passengers may be distracted. This is disadvantageous for safety reasons.

[0047] However, as described above, by a special design of the coating with open pores having preferably continuous porosity, the components of the polymer layer can at least partially fill these pores. Here, "components of the polymer layer" does not mean that the individual components of the polymer layer enter the pores, but that the polymer layer is partially introduced into the pores and at least partially fills these pores. This can occur, for example, if the polymer layer is arranged between the glass sheets, for example in the form of a film, during the formation of the glass composite, and during the lamination process the viscosity of the polymer layer is reduced so that the polymer layer is introduced into the pores due to capillary forces. According to one embodiment, this can occur in the form that the pores are essentially completely filled with the polymer layer, i.e. at least 80 vol%, preferably more than 80 vol% of the pores are filled with the polymer layer. However, it is generally difficult to produce composite glasses whose filling degree can be determined analytically.

[0048] In this case, by filling the pores with a polymeric (or plastic) material, a uniform, very dark color coordinate can surprisingly be achieved even if the polymer of the polymer layer itself is not colored. This eliminates the need to use two different polymer layers, namely a colored polymer layer for the area of ​​the at least one coating and an uncolored / transparent polymer layer in the "visible area" of the composite glass. This greatly simplifies the production of the composite glass.

[0049] In this way, color coordinates of the composite glass in the CIEL*a*b* system can be achieved very simply, which color coordinates are measured in at least one area of ​​at least one coating applied to the second side of at least one glass sheet along the observation direction from the first side to the second side of the at least one glass sheet, wherein L* is at most 12 and preferably at least 1, and a* and b* are both in the range between +5 and -5.

[0050] Preferably, the polymer layer contains polyvinyl butyral (PVB) or is formed, for example, as a so-called PVB film.

[0051] According to one embodiment, the thickness of the polymer layer may be between 650 μm and 850 μm. Typical thicknesses of exemplary suitable films are, for example, between 700 μm and 760 μm.

[0052] According to another embodiment, the at least one coating may have a thickness between 2 and 10 μm, for example at most 7 μm.

[0053] Preferably, the at least one sheet comprising borosilicate glass may be a float glass sheet. In this case, the at least one coating is preferably applied on the so-called atmosphere side of the glass sheet.

[0054] According to one embodiment, the light transmittance τ measured in at least one region is vis Less than 5%, preferably less than 2%, more preferably less than 1%, particularly preferably less than 0.5%. Of course, this transmittance is achieved when at least one coating is applied over the entire surface. The lower transmittance indicates that, according to this embodiment, the at least one coating has a very high light-shielding and laminating effect.

[0055] It is generally noted that the at least one coating is usually applied around the edge of at least one glass pane and in a corresponding manner around the edge of the composite glass. It can be provided that in certain areas, for example in the area where the rearview mirror is mounted on the windshield, for example, there can be projections. It can also be provided that in the area facing the inside of the composite glass, the frame applied over the entire surface transitions into an area with a certain coverage, in which the coating is applied in the form of a grid with a lower coverage. This is very common, for example, in the case of windshields of vehicles.

[0056] According to one embodiment, the pigment content of the at least one coating is between 1 vol% and 40 vol%, preferably less than 37.5 vol%, wherein the preferred lower limit is usually 5 vol%. In this way, an optically tinted dark coating can be achieved while also ensuring sufficient adhesion strength of the coating on the substrate (here, the glass plate).

[0057] According to another embodiment, this is advantageously achieved in that the glassy component content of the at least one coating is between 60 vol% and 99 vol%, preferably between 62.5 vol% and 95 vol%, relative to the solid content of the at least one coating. The solid content of less than 100 vol% can be formed in particular by at least one pigment, for which further components such as one or more fillers and further pigments can be used as required.

[0058] If the composition of the at least one coating is not given in vol % but in wt %, the pigment content of the at least one coating is between about 1 wt % and 60 wt %. The glass content of the at least one coating is between about 35 wt % and about 98 wt %. If the at least one coating contains additives designed as fillers, their content by weight can be between 1 wt % and 15 wt %. These statements, as well as the statements about volume percentages, relate to the solids content of the at least one coating and therefore also apply accordingly to the solids content of the slurry, which can be used to produce the corresponding at least one coating of the glass sheet according to the embodiment.

[0059] According to another embodiment, in addition to at least one pigment and the glassy component, the at least one coating also contains an additive. Of course, the at least one coating may also contain a variety of additives formed in different ways. The additive may, for example, be designed as a filler, for example, a filler designed to improve scratch resistance or to influence the thermal expansion of the coating. The additive may also be a foaming agent, which may also be referred to as a pore former or a foaming agent. Such a foaming agent decomposes when the at least one coating is fired, wherein a gas is formed, which contributes to the formation of pores and in particular also advantageously supports the formation of open porosity, which is particularly advantageous here. The additive designed as a foaming agent may be added to the slurry for manufacturing the at least one coating according to the embodiment in a corresponding amount, just like the additive designed as a filler, but for obvious reasons (i.e. decomposition), it is no longer included in the solid content of the at least one coating.

[0060] According to another embodiment, the glassy component of the at least one coating comprises, in wt% (weight percentage) of oxides:

[0061] SiO 2 10 to 70

[0062] B 2 O 3 5 to 30, preferably 6 to 25.

[0063] In other words, the vitreous component (or glass flow or glass powder) according to this embodiment itself is formed to include borosilicate glass. This is obviously advantageous because it enables a higher compatibility between the glass flow and the at least one glass sheet to which the at least one coating is locally applied.

[0064] Furthermore, it can generally be assumed that the glassy component still contains Al 2 O 3 , and its content is preferably less than 10wt%.

[0065] According to other preferred embodiments, the glass flow or the glassy component can be formed in different ways in the frame, depending on the specific center of gravity.

[0066] For example, the glassy component of at least one coating layer may comprise, by weight percent of oxides: SiO 2 10 to 50

[0067] B 2 O 3 10 to 26

[0068] ZnO 20 to 50,

[0069] Among them, preferably, the alkali metal oxide (R 2 The sum of the oxides of metals O) is between less than 0.5 wt % and 10 wt %, and / or the sum of the alkaline earth metal oxides is between 0 wt % and 2.5 wt %.

[0070] In this case, the glass stream is thus formed as a zinc borate glass stream. This is advantageous because it reduces the melting temperature of the glass powder, thereby ensuring sufficient fluidity at the firing temperature (500-750° C.), regardless of the pigment and filler content.

[0071] According to another embodiment, the glassy component of at least one coating comprises, in wt% of oxides: SiO 2 30 to 60

[0072] B 2 O 3 15 to 25

[0073] Bi 2 O 3 8 to 45,

[0074] Among them, preferably, the alkali metal oxide (R 2O) is between 3.5 wt% and 8.5 wt%, preferably between 4 wt% and 6.5 wt%, and / or the sum of alkaline earth metal oxides is less than 0.5 wt%. Preferably, according to this embodiment, the glassy component comprises at least 2.5 wt% of a selected from Li 2 O、Na 2 O and K 2 O, wherein the alkali metal oxide (R 2 The ratio of O) to alumina is usually less than 6, i.e.

[0075]

[0076] In this case, it is therefore a bismuth borate glass stream. This is particularly advantageous if an optimum is to be achieved between the thermal expansion coefficients of substrate and glass stream, taking into account the firing temperature. This allows particularly good strength values ​​to be achieved.

[0077] According to another embodiment, the glassy component comprises, by wt% of oxides: SiO 2 50 to 70

[0078] B 2 O 3 15 to 30

[0079] Bi 2 O 3 0 to 15

[0080] ZnO 0 to 5,

[0081] Preferably, the total amount of alkali metal oxides is between 4 and 6.5 wt %, and / or the total amount of alkaline earth metal oxides is between 0 and 2.5 wt %.

[0082] According to a further embodiment, the at least one coating comprises an additive designed as a filler, wherein the linear thermal expansion coefficient of the filler is preferably in the range of -7*10 -6 / K to 1.5*10 -6 / K. The linear coefficient of thermal expansion may also be referred to as α, wherein the temperature range for determining the coefficient of expansion may also be given as an index. In the context of the present disclosure, if thermal expansion is mentioned, linear thermal expansion is meant. In the context of the present disclosure, unless expressly stated otherwise, the terms "linear coefficient of thermal expansion", "coefficient of thermal expansion", "coefficient of expansion", "CTE" and "α" are used synonymously. In particular, the method according to ISO 7991 may be used to determine the linear coefficient of thermal expansion.

[0083] Fillers with a coefficient of thermal expansion in the above range are advantageous because they can influence and in particular reduce the thermal expansion of at least one coating layer caused by its components. Since the coefficient of thermal expansion of pigments is usually relatively higher than that of borosilicate glass as substrate material according to the present disclosure, fillers with a relatively low coefficient of thermal expansion can be added to the coating layer to advantage, so that the strength of the resulting glass sheet / composite is not too low.

[0084] According to one embodiment, it has been shown that, when adding fillers, a glass sheet composite with good mechanical properties and high opacity can be obtained by specifically adjusting the ratio of the pigment and nanoparticle filler content. The diameter of the pigment used is usually at least one order of magnitude larger than the diameter of the nanoparticle filler. The preferred diameters or sizes of these pigments are also given further in the example section below.

[0085] According to one embodiment, said at least one coating comprises additives in the form of fillers in a content between 0.5 vol% and 20 vol%, preferably less than 15 vol%.

[0086] Preferably, it can be provided that the at least one coating can have two fillers, which have different properties, for example, in terms of their particle size. In this case, with respect to the particle size, the d 50 For values, the equivalent diameter is always considered. Therefore, unless otherwise explicitly stated, if "particle size" or "diameter" is generally mentioned in the context of the present disclosure, it refers to the d of the particle size distribution. 50 value.

[0087] This embodiment with two fillers of different particle sizes can be advantageous, since it can produce a particularly advantageous pore size distribution, whereby in particular the polymer can be diffused or infiltrated into the pores of at least one coating in a particularly simple manner. For example, one filler can be a nanofiller, i.e. a filler with a particle size of less than 100 nm, but the particle size of the other filler is at least half an order of magnitude larger than the nanoparticle filler. The particle size of the nanoparticle filler can be, for example, up to 50 nm, wherein in this case the particle size of the other filler should advantageously be, for example, at least 0.5 μm. In this way, a good porosity in the coating can be achieved particularly well. Typical sizes for non-nanoparticle fillers are approximately 0.5 μm to 1.5 μm.

[0088] However, it has been shown that when adding preferred nanoparticulate fillers (i.e. fillers with a particle size of not more than 50 nm), it may even be sufficient to adjust only the content ratio of pigment to nanoparticulate filler if no other fillers are present. This is because the diameter of the pigment used is usually at least one order of magnitude larger than the diameter of the nanoparticulate filler. For white pigments, the diameter is preferably less than 1 μm, preferably less than 0.8 μm, particularly preferably less than 0.6 μm. Preferred diameters or sizes of these pigments are also given further below in the Examples section.

[0089] According to another embodiment, the at least one coating and / or the slurry comprises another additive designed as a blowing agent. In this case, the blowing agent content in the slurry with which the respective at least one coating according to the embodiment for the composite glass according to the present disclosure can be produced is preferably between 5 vol% and 25 vol%, particularly preferably less than 15 vol%.

[0090] According to another embodiment, the at least one glass sheet comprises: at least 60 wt % and at most 85 wt % SiO 2 ; at least 8 wt% and at most 26 wt% B 2 O 3 ; at least 0.5wt% and at most 12wt% Al 2 O 3 ; and at least 0.5 wt% and at most 6 wt% of Na 2 O, which may preferably also contain up to 1 wt % of Li 2 O; up to 4 wt% K 2 O; up to 5wt% MgO; up to 3.5wt% CaO; up to 4wt% SrO; up to 3wt% ZnO; up to 3wt% ZrO 2 ; and other minor components, such as refining agents, wherein the sum of these minor components does not exceed 2wt%.

[0091] SiO 2 is the main network former and is the main component of the glass of the at least one glass sheet. Therefore, in order to ensure that the glass sheet has sufficient chemical and mechanical stability, SiO in the glass sheet 2 The content should be at least 60 wt%. However, in order to ensure good meltability, the SiO 2 The content is preferably limited, and according to one embodiment, does not exceed 85 wt%. B 2 O 3 B is another component of the at least one glass sheet, and its content in the glass is preferably at least 8 wt %. In this way, the melt viscosity of the glass can be kept at a low level, which is advantageous from a production point of view. 2 O3 The content should not be too high in order to obtain glass with sufficient chemical stability. In addition, the glass also contains at least 0.5wt% Al 2 O 3 .Al 2 O 3 Al is a so-called intermediate oxide which is preferably added to borosilicate glasses in order to reduce the segregation tendency in these glasses. 2 O 3 It can also improve the hardness of glass. However, due to Al 2 O 3 At the same time, it may reduce chemical resistance and increase melting temperature. Therefore, Al in glass 2 O 3 The content should not be too high, and the preferred upper limit here is at most 12 wt %. Finally, the glass also contains at least 0.5 wt % and at most 6 wt % of Na 2 O. In this way, the melting point of the glass can be further reduced while ensuring that Na 2 The O content will not be too high, and the Na 2 The O content significantly reduces the chemical resistance of the glass.

[0092] The glass may also contain other components. For example, up to 1 wt% of Li 2 O, up to 4 wt% K 2 O, up to 5 wt% MgO, up to 3.5 wt% CaO, up to 4 wt% SrO, up to 3 wt% ZnO, up to 3 wt% ZrO 2 These components can affect different properties of the glass, for example further counteracting the segregation tendency (such as adding K 2 O), improve the strength of glass, etc.

[0093] Of course, the glass may generally contain other minor components, such as refining agents, wherein the sum of these minor components does not exceed 2 wt %.

[0094] According to a further embodiment, the further glass pane comprises or consists of soda-lime glass.

[0095] Soda-lime glass usually contains SiO 2 , CaO and Na 2O is the main component of glass and is produced in large quantities. It is inexpensive, but also has certain disadvantages, such as relatively low chemical resistance and mechanical stability. However, based on easy availability, this glass can be used particularly advantageously for composite glass, and more specifically, it is preferably used on the side of the composite body that is exposed to less mechanical load and / or corrosion during use. In the case of a vehicle window made of or including composite glass, the side may advantageously be the side of the composite glass facing the interior of the vehicle. This achieves a good compromise between good durability of the composite glass and acceptable costs.

[0096] According to another embodiment, the composite body achieves at least level 3 in the so-called impact test. The impact test is a measure of the durability or quality of the composite body and is described in the ASTM C1908-21 standard. Generally speaking, when a composite body (which can also be referred to as "composite safety glass") is damaged, the glass fragments must adhere to the polymer layer, for example in the form of a PVB film, which is located between the glass sheets of the composite body. This is checked with the help of an "impact test", in which a composite glass comprising two glass sheets and having a maximum thickness of 2*4 mm is handled, i.e. struck, with a hammer on an inclined metal base. In this case, the glass is damaged by the mechanical action. A visual inspection is then carried out. For each exposed film face or each exposed surface of the polymer layer, the adhesion level is divided into "impact values" between 0 and 10, wherein a higher value means that the glass fragments adhere better to the polymer layer.

[0097] The present disclosure also generally relates to a method for producing a glass sheet comprising at least one coating and / or for producing a composite body comprising a glass sheet comprising at least one coating.

[0098] In order to produce a glass sheet comprising at least one coating, a slurry can generally be used which comprises a glass stream, at least one pigment and preferably at least one additive, the at least one additive preferably being in the form of a filler. In this case, the above statements about the composition of at least one coating according to the embodiment should apply accordingly with regard to the content of pigments and binders, that is, the information about the contents is related to the solid content of the slurry. In addition to the corresponding solid content in a corresponding amount, the slurry generally also comprises about 30 wt % to 45 wt % of a medium or dispersion medium, generally a high-boiling solvent or a solvent mixture. In particular, when the slurry is applied to the glass sheet by screen printing, the slurry can in particular be a so-called "screen printing oil".

[0099] The paste may be applied by conventional coating processes, in particular by a printing process such as screen printing.

[0100] Furthermore, the slurry may also contain additives in the form of foaming agents.

[0101] Preferably, the composition of the slurry, in particular with regard to at least one vitreous component, and of the glass used in the glass sheet to which the at least one coating is or is to be applied is coordinated with one another so that, in the case of bending of the glass sheet, the firing temperature and time of the at least one coating preferably correspond to the bending temperature and time of the sheet. From a viscosity point of view, the formation of the at least one coating designed as a porous glaze layer is carried out at a temperature at which the viscosity of the sheet lg [η] / dPas is 8-11, preferably 9-10, i.e. preferably at a temperature of at least 590° C. and at most 850° C.

[0102] Example

[0103] In the following table, some compositions suitable for glass sheets according to embodiments of the present disclosure are listed along with relevant data on the properties achieved using these glass compositions. These compositions are all calculated in wt% of oxides.

[0104] Deviations from 100% in the sum result from rounding of the analytical results.

[0105]

[0106]

[0107] Exemplary compositions of suitable glass streams can be found in the table below. These compositions are also given here in wt %. Any deviations from the sum of 100 wt % are due to rounding.

[0108]

[0109] The following table lists suitable pigments for the coating according to the embodiments. The given pigment class is associated with a so-called "color index", wherein the pigments are divided into several classes, wherein in the table, "Bk" stands for "black", "Br" stands for "brown", and "Gr" stands for "green". In this case, the pigments listed are generally suitable for producing dark coatings according to the embodiments, in particular also for producing coatings that produce a black color impression. This also applies in particular to pigments classified as "brown" or "green" in the table, since these pigments are generally composed so that they have a strong adsorption, and in coatings containing these pigments, the "color" (if present) usually only appears in the form of a lighter shade (as brown-black or dark green), and the overall color impression of such a coating is dark or black.

[0110]

[0111]

[0112] Suitable additives for the slurry or coating according to the embodiment can be found in the following table:

[0113]

[0114]

[0115] In the case of fillers, particularly suitable are low-stretch fillers such as those listed in the table above, for example silicic acid. In this case, the silicic acid can be used in different variants, for example as silicic acid with a rather compact but small particle shape (silicic acid (1) in the table above), or in the form of silicic acid with a particularly large surface area (silicic acid (2) in the table above). It is also common to use amorphous or crystalline fillers that are porous in themselves, such as the "CoralPor" fillers mentioned above. These fillers are fillers made of porous borosilicate glass. Other fillers are also conceivable, such as porous and crystalline zeolites, or other low-stretch fillers other than β-eucryptite, such as cordierite. In this case, the addition of fillers is also very effective in increasing the double ring bending strength; compared to a slurry / coating of the same composition but without filler, even if only 1.75 vol% (relative to the resulting coating) of filler is added, the strength (double ring bending tensile strength) is increased by 12.5% ​​to 14.5%. In this case, the fillers used are "silicic acid (1)", β-eucryptite and filler.

[0116] Inorganic and organic foaming agents can generally be used, with organic foaming agents being preferred, as described above, for example sugars (maltose, glucose, etc.) or starch. If such foaming agents (or pore formers) are added, then in addition to the positive effect on the color, the strength of the glass sheet and the corresponding resulting composite is also increased (double loop bending tensile strength) by more than 40% (starch as foaming agent / pore former) or more than 30% (sugars) compared to a coating of the same composition but without pore former / foaming agent. In this case, 10 vol% of pore former / foaming agent is added to the slurry. This results in an increase in the pores in the coating by 10 vol% compared to the case without the addition of a foaming agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0117] The present invention will be further described below in conjunction with the accompanying drawings. The accompanying drawings show:

[0118] Figure 1 is a schematic, not-to-scale, diagram of a section through a composite glass according to one embodiment;

[0119] Figure 2 is a schematic diagram not drawn to scale of a glass sheet according to one embodiment;

[0120] Figure 3is a schematic top view not drawn to scale of a composite glass according to an embodiment;

[0121] Figures 4 to 7 are scanning electron micrographs of glass sheets having at least one coating in laminated and unlaminated states. DETAILED DESCRIPTION

[0122] Figure 1 1 is a schematic diagram not drawn to scale of a composite or composite glass 10 according to an embodiment of the present disclosure. The composite glass 10 comprises two glass panes 1, 2. The pane 1 shows at least one glass pane having at least one locally applied coating. The pane 2 is another glass pane and can be made of soda-lime glass, for example. A polymer layer 3 is arranged between the two glass panes 1, 2 and a coating 11 is arranged in the edge region of the composite glass 10. The polymer layer is arranged on one side (not shown) of the glass pane 1 and in the following description, the polymer layer can include at least one coating, or can include at least one coating and optionally another coating as an intermediate layer.

[0123] For better illustration, the coating 11 is shown here as thicker, i.e. as comparable to the thickness of the two plates 1, 2; however, as mentioned above, this is only for better illustration. The coating 11 is usually significantly thinner than either of the two plates 1, 2 and is usually also thinner than the polymer layer 3. The polymer layer 3 can also be a film. An exemplary thickness of the polymer layer is between 650 and 850 μm, wherein the thickness of at least one coating is usually in the single-digit micrometer range. The preferred upper limit of the layer thickness of the at least one coating is, for example, 7 μm or 6 μm. In addition, the thickness of at least one coating can be, for example, between 3 μm and 5 μm.

[0124] As shown in the figure, the composite glass 10 is formed as a curved composite glass pane, which can also be used as a windshield, for example. Figure 1 In the example shown, the composite glass 10 may also not include curved panels 1, 2, but may be formed in a flat manner. The curvature of the composite glass 10 may also be related to Figure 1 The opposite is true. Figure 1 In the example shown, the glass sheet 1 is the outer side of the windshield, however, in general, the glass sheet 1 can also be arranged on the inner side of the windshield. However, in any case, the coating 3 is arranged between the two glass sheets 1, 2.

[0125] However, according to Figure 1is preferred, since in this way the first glass pane 1, for example when used as a windshield, is exposed to stone chips or chemical loads (e.g. salt spray), to which a glass pane made of borosilicate glass can withstand better than, for example, commercially available soda-lime glass panes. However, as mentioned above, for cost reasons it is advantageous if both panes of the composite glass do not contain borosilicate glass.

[0126] Therefore, Figure 1 The arrangement shown may be advantageous because the glass sheet 1 comprises SiO 2 and B 2 O 3 As a component of the vitreous material. Such borosilicate glass is more scratch-resistant than soda-lime glass, for example, and therefore it may be advantageous if the glass sheet 1 is Figure 1 The composite 10 is shown formed so that the glass pane 1 faces "outward", ie outwards when used as a windshield. This allows for better protection against stone chips and similar mechanical loads.

[0127] To explain the structure of the glass plate 1 according to the embodiment, Figure 2 The glass sheet 1 is shown in the form of a schematic diagram drawn true to scale. Figure 2 However, the glass sheet 1 is not yet bent. Figure 1 , which can also be bent. However, it may be advantageous to first use an unbent flat plate 1 and then bend it, for example in a thermal process. Here, too, the thickness of the coating 11 is shown to be significantly greater than the actual thickness for the sake of illustration.

[0128] The layout of plate 1 and Figure 1 The arrangement shown corresponds to Figure 2 The plate in the composite body is not bent. As shown in the figure, the coating 11 is formed on the side 102 facing the second plate 2 in the composite body 10. The polymer layer 3 is not shown here, which is arranged between the plate 1 and the plate 2 in the composite body. It should be clearly pointed out here that the polymer layer 3 is both in direct contact with the side 102 of the plate and is arranged on the coating 11 provided in the area of ​​the plate 1 (or the side 102 of the plate 1).

[0129] The coating 11 is arranged in the edge region of the plate 1, namely in each Figure 2 The left and right sides in the illustrated diagram. Here, the coating can be applied in the form of a "frame", for example.

[0130] In this regard, refer to Figure 3 , Figure 3A view of a composite glazing 10 according to an exemplary embodiment is also shown in a schematic diagram, not drawn to scale. The coating 11 is formed here as a circumferential frame around the edge of the pane 1, wherein the coating is initially formed in a decked manner, thus as an uninterrupted layer, and transitions to an uncoated area towards the center of the pane 1 via a grid or dot pattern 111. When the pane 1 is used in a composite glazing 10, this uncoated area is, for example, a visible area of ​​a windshield. Of course, in general, this frame may not be as Figure 3 It is not formed uniformly as schematically shown in the figure, but has, for example, a projection, as is usually the case on a windshield in the area of ​​a rearview mirror.

[0131] Figure 4 and Figure 6 is a scanning electron micrograph of a partially coated glass sheet according to an embodiment of the present disclosure, wherein the glass sheet includes a SiO 2 and B 2 O 3 The glass sheets have a first side and a second side.

[0132] Here, the coating is usually at least one coating applied in at least one region of the second side of the glass pane. The coating is usually formed as an enamel coating, which includes at least one pigment, a glass component and preferably at least one additive, such as a filler.

[0133] from Figure 4 and Figure 6 As can be seen in the illustration shown, at least one coating comprises pores, preferably open pores. Thus, the at least one coating preferably results in a direct connection between a side of the at least one coating facing the second side of the at least one glass sheet and a side of the at least one coating facing away from the second side of the at least one glass sheet.

[0134] from Figure 5 and Figure 7 (in Figure 5 for Figure 4 The laminated samples, Figure 7 for Figure 6 It can be seen from the illustration of the laminated sample in FIG. 1 that during the lamination process, the polymer layer at least partially penetrates into the pores of at least one coating layer.

[0135] Reference numerals list

[0136] 1 glass plate 10 Composite, composite glass 11 coating 101、102 Side of glass panel 111 Dot Grid 2 Another glass plate 3 Polymer layer.

Claims

1. A composite glass, particularly for a vehicle, the composite glass include: Two glass sheets, at least one of which is partially coated and comprises SiO 2 and B 2 O 3 a glass sheet of glass having a first side and a second side, at least one coating applied in at least one region of said second side of said at least one glass sheet, wherein the at least one coating is formed as an enamel coating which comprises at least one pigment, a glass component and preferably at least one additive, in particular a filler, wherein the at least one coating comprises pores, preferably open pores, so that in the at least one coating a direct connection preferably occurs between a side of the at least one coating facing the second side of the at least one glass pane and a side of the at least one coating facing away from the second side of the at least one glass pane, Preferably, the at least one glass sheet has a bending strength of at least 5 MPa to at most 170 MPa, preferably at least 20 MPa to at most 170 MPa, more preferably at least 35 MPa, particularly preferably at least 60 MPa, most preferably at least 80 MPa, The composite glass further comprises at least one polymer layer arranged between the glass panes, wherein the polymer of the polymer layer is present in an uncolored manner and wherein in the region of the at least one coating at least a portion of the polymer layer at least partially fills pores of the at least one coating, This results in color coordinates of the composite glass in the CIEL*a*b* system, which are measured in the viewing direction from the first side to the second side of the at least one glass sheet in at least one area where the at least one coating is applied to the second side of the at least one glass sheet, wherein L* is at most 12 and preferably at least 1, and a* and b* are both in the range between +5 and -5.

2. The composite glass according to claim 1, in, The light transmittance τ measured in the at least one region vis Less than 5%, preferably less than 2%, more preferably less than 1%, particularly preferably less than 0.5%.

3. The composite glass according to claim 1 or 2, comprising at least one of the following features: - the pigment content of the at least one coating is between 1 vol% and 40 vol%, preferably less than 37.5 vol%, wherein the preferred lower limit is usually 5 vol%, - the glassy component content of the at least one coating is between 60 vol% and 95 vol%, based on the solid content of the at least one coating.

4. The composite glass according to any one of claims 1 to 3, in, The glassy component of the at least one coating comprises, in wt% of oxides: SiO 2 10 to 70 B 2 O 3 5 to 30, preferably 6 to 25.

5. The composite glass according to claim 4, in, The glassy component of the at least one coating comprises, in wt% of oxides: SiO 2 10 to 50 B 2 O 3 10 to 26 ZnO 20 to 50, Wherein, preferably, the sum of alkali metal oxides is between less than 0.5wt% and 10wt%, and / or the sum of alkaline earth metal oxides is between 0wt% and 2.5wt%; or SiO 2 30 to 60 B 2 O 3 15 to 25 Bi 2 O 3 8 to 45, Wherein, preferably, the sum of alkali metal oxides is between 3.5 wt % and 8.5 wt %, particularly preferably between 4 wt % and 8 wt %, and / or the sum of alkaline earth metal oxides is less than 0.5 wt %; or SiO 2 50 to 70 B 2 O 3 15 to 30 Bi 2 O 3 0 to 15 ZnO 0 to 5, Preferably, the total amount of alkali metal oxides is between 4 wt % and 6.5 wt %, and / or the total amount of alkaline earth metal oxides is between 0 wt % and 2.5 wt %.

6. The composite glass according to any one of claims 1 to 5, in, The at least one coating layer comprises an additive in the form of a filler, wherein the linear thermal expansion coefficient of the filler is preferably in the range of -7*10 -6 / K to 1.5*10 -6 / K.

7. The composite glass according to any one of claims 1 to 5, in, The at least one coating layer comprises an additive in the form of a filler, the content of the filler being between 0.5 vol% and 20 vol%, preferably less than 15 vol%.

8. The composite glass according to any one of claims 1 to 7, in, The at least one glass sheet comprises: at least 60 wt % and at most 85 wt % SiO 2 ; at least 8 wt% and at most 26 wt% B 2 O 3 ; at least 0.5wt% and at most 12wt% Al 2 O 3 ; and at least 0.5 wt% and at most 6 wt% of Na 2 O, wherein the at least one glass pane can preferably also contain: up to 1 wt % Li 2 O; up to 4 wt% K 2 O; up to 5wt% MgO; up to 3.5wt% CaO; up to 4wt% SrO; up to 3wt% ZnO; up to 3wt% ZrO 2 and other minor components, such as refining agents, wherein the sum of these minor components does not exceed 2wt%.

9. The composite glass according to any one of claims 1 to 8, in, The other glass pane comprises or consists of soda-lime glass. 10 . The composite glass according to claim 1 , which has a result of at least 3 in the so-called impact test.