Bending-resistant and pressure-resistant diaphragm pump diaphragm and preparation method thereof

By adopting a combination of materials with specific ratios and hot pressing treatment in the diaphragm pump diaphragm, the problem of poor resistance to bending and dynamic fatigue of the existing diaphragm is solved, the compression and bending ability of the diaphragm is improved, and the use is extended. Lifespan and reduce maintenance costs.

CN119017796AActive Publication Date: 2024-11-26KUNSHAN YUSI XIANGJIE AUTOMATION TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411095439.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing diaphragm pump diaphragms have poor resistance to bending dynamic fatigue in harsh media environments, short service life, and are not resistant to ketones, ethers, esters and other organic solvents.

Method used

Using a diaphragm pump diaphragm including elastic side body, pressure resistant intermediate and wear-resistant surface body, the combination of materials such as ternary fluoroelastomer, fiber braided mesh fabric, matrix resin and surface modified nanoTiO2, is adopted. Compounding and hot pressing treatment are carried out to enhance the compression and bending resistance of the diaphragm.

Benefits of technology

It significantly improves the bending resistance and fatigue resistance of the diaphragm pump diaphragm, extends the service life, reduces maintenance and maintenance costs, and maintains good performance in a variety of media environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of diaphragm pump diaphragm preparation, and discloses a bending-resistant and pressure-resistant diaphragm pump diaphragm which comprises an elastic side body and a pressure-resistant intermediate. According to the preparation method of the flexure-resistant and pressure-resistant diaphragm pump diaphragm, the diaphragm pump diaphragm has excellent flexure resistance, fatigue resistance and resistance to various media, can keep high breaking strength and elongation at break in the environments of media such as esters and ketones, and has good reciprocating flexure resistance, fatigue resistance and compression set performance; the diaphragm pump has an excellent anti-corrosion effect when applied to the diaphragm pump, the pressure-resistant middle body, the elastic side face body and the wear-resistant surface body are overlapped from inside to outside, the fiber woven grid fabric is wrapped in the diaphragm body, and the fiber woven grid fabric is subjected to enhancement treatment, so that the pressure resistance and flexing resistance of the diaphragm pump are greatly improved, and the service life of the diaphragm pump is prolonged. The combination of the elastic side body and the wear-resistant surface body further improves the flexing resistance of the diaphragm pump diaphragm, effectively prolongs the service life of the diaphragm pump diaphragm, and reduces the repair and maintenance cost of the diaphragm pump.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diaphragm pump diaphragm preparation, in particular to a diaphragm pump diaphragm that is resistant to bending and pressure and a preparation method thereof. Background Art

[0002] The diaphragm pump is a special type of positive displacement pump. It relies on the back and forth movement of a diaphragm to change the volume of the working chamber to inhale and discharge liquid. The diaphragm pump is mainly composed of two parts: the transmission part and the diaphragm cylinder head. The transmission part drives the diaphragm to move back and forth through hydraulic transmission. The liquid being transported is separated from the working liquid by the diaphragm in the pump cylinder, and only contacts the pump cylinder, the suction valve, the discharge valve and the pump side of the diaphragm, but not the plunger and the sealing device. This allows the plunger and other important parts to work completely in the oil medium and be in good working condition; Fluorine-containing rubber refers to a synthetic polymer material containing fluorine atoms on the main chain or side chain carbon atoms. Due to the extremely high electronegativity of fluorine atoms, the CF bond energy is relatively large. At the same time, its atomic radius is equivalent to half of the CC bond, and it can be closely arranged around the carbon atoms, which plays a good volume shielding role for the main chain carbon atoms, giving fluorine rubber good chemical stability and physical and mechanical properties. It can be widely used in aerospace, aviation, military industry, national defense, automobile and other fields, especially in sealing. The diaphragm is one of the most important core components of the diaphragm pump, which is required to have good flexibility and excellent corrosion resistance. However, the medium conveyed by the diaphragm pump is usually of very poor quality, resulting in the life of the diaphragm in actual use being generally lower than the design life of the diaphragm pump. At the same time, when the hydraulic diaphragm pump is working, the central diaphragm swings back and forth continuously, and is subjected to the test of flex fatigue; In the prior art, fluororubber as a seal has poor dynamic fatigue resistance to flexing, and is damaged after about 10,000 flexing times; its chemical properties are relatively stable, and it can withstand most organic and inorganic solvents and most petroleum-based oils, but it is not resistant to organic solvents such as ketones, ethers, and esters. When it is in various media environments for a long time, the mechanical properties and strength of fluororubber are low. When used as a diaphragm in a diaphragm pump, it is easily damaged and has a short service life; Therefore, the present invention provides a diaphragm pump diaphragm that is resistant to bending and pressure and a preparation method thereof to solve the above-mentioned problems. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a diaphragm pump diaphragm that is resistant to bending and pressure and a preparation method thereof, which has the following advantages and solves the above-mentioned problems.

[0004] To achieve the above object, the present invention provides the following technical solution: a bending and pressure-resistant diaphragm pump diaphragm, comprising an elastic side body, a pressure-resistant intermediate body and a wear-resistant surface body; The elastic side body comprises the following raw materials in proportion by weight: 60-80 parts of ternary fluororubber, 6-8 parts of crosslinking aid, 1-6 parts of dispersant, 2-8 parts of accelerator, 5-10 parts of vulcanizing agent, 40-53 parts of fiber woven mesh fabric, 6-9 parts of toughening agent, and 16-19 parts of elastomer; The pressure-resistant intermediate comprises the following raw materials in the following weight proportions: 80-117 parts of base resin, 30-60 parts of reinforcement, and 16-48 parts of support; The wear-resistant surface body comprises the following raw materials in the following weight proportions: 40-45 parts of base material, 10-15 parts of surface material, 6-18 parts of antioxidant, and 2-8 parts of surface modification material.

[0005] Preferably, the cross-linking aid is triallyl isocyanurate, the dispersant is a mixture of urea and glycerol, the antioxidant is one of antioxidant MB, antioxidant A, and antioxidant D, the accelerator is one or more of accelerator DM, accelerator D, accelerator M, accelerator TT, and accelerator CE, and the vulcanizing agent is sulfur.

[0006] Preferably, the elastomer is TPE elastomer particles, and the fiber woven mesh fabric is PET long fiber woven mesh fabric.

[0007] Preferably, the toughening agent is one of an MBS toughening agent and an AK toughening agent.

[0008] Preferably, the matrix resin is one of silicone rubber, PERT or HDPE resin powder, and the reinforcement is one of potassium hexatitanate whiskers and aluminum borate whiskers or a mixture of the two.

[0009] Preferably, the support is a carbon nanotube, and the carbon nanotube is at least one of a zigzag nanotube, an armchair nanotube and a helical nanotube.

[0010] Preferably, the surface modification material is modified nano-TiO2; The surface-modified nano-TiO2 is surface-modified nano-TiO2 prepared by a sol-gel method. 10 ml of butyl titanate is slowly dripped into 35 ml of anhydrous ethanol at room temperature, stirred for 10 minutes and then allowed to stand to form a yellow clear solution. Then 2 ml of glacial acetic acid and 10 ml of anhydrous ethanol are mixed, and vigorously stirred to obtain a transparent solution. Then hydrochloric acid is dripped into the solution to adjust the pH value to 3. In a room temperature water bath, the yellow clear solution is dripped into the transparent solution under vigorous stirring to obtain a light yellow solution. Then, the solution is heated in a water bath at 40°C with stirring for 1 hour to obtain a white gel. Then, the gel is dried at 80°C, and then heat-treated at 600°C for 2 hours to obtain a white nano-TiO2 powder. Finally, the obtained white nano-TiO2 powder is blended and stirred with sodium dodecyl sulfate for 40 minutes, and the surface-modified nano-TiO2 is obtained after drying.

[0011] Another technical problem to be solved by the present invention is to provide a method for preparing a diaphragm pump diaphragm that is resistant to bending and pressure, comprising the following steps: Step 1: Preparation of elastic side body: Prepare appropriate weight proportions of ternary fluororubber, crosslinking aid, dispersant, accelerator, vulcanizing agent, fiber woven mesh fabric, toughening agent, and elastomer; Step 2: After mixing the ternary fluororubber with the elastomer, toughening agent and dispersant, the mixture is put into an open mill, and a vulcanizing agent is added, and thin-pass refining is performed in the open mill; Step 3: Then the rubber material after the open mixing is placed in a three-roll calendering device for calendering to obtain a film, the distance between the second roll and the third roll is smaller than the distance between the first roll and the second roll, and the film is cut using a slitting machine; Step 4: The fiber woven mesh fabric is then stored, unrolled, flattened, and rolled and laminated with the diaphragm, and the cross-linking aid and accelerator are evenly added. After the lamination, it is introduced into the drying tunnel assembly line, and heated in the drying tunnel assembly line to vulcanize and foam the diaphragm until the diaphragm is completely in a creeping state. The fiber woven mesh fabric is hot-pressed and laminated with the diaphragm layer, flattened, and then punched; Step 5: Preparation of pressure-resistant intermediate: Prepare appropriate weight proportions of matrix resin, reinforcement and support; Step 6: fully mix the matrix resin, reinforcement and support, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step 7: Preparation of wear-resistant surface body: Prepare appropriate weight proportions of base material, fabric, antioxidant and surface modifier; Step 8: fully mix the base material, fabric, antioxidant and surface modification material, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step nine: overlap the prepared pressure-resistant intermediate body, elastic side body and wear-resistant surface body in order from inside to outside, introduce them into the drying tunnel assembly line after compounding, perform hot pressing compounding, flatten, and then punch out.

[0012] Compared with the prior art, the present invention provides a bending and pressure-resistant diaphragm pump diaphragm and a preparation method thereof, which has the following beneficial effects: 1. The preparation method of the bending and pressure-resistant diaphragm pump diaphragm makes the diaphragm pump diaphragm have excellent bending and fatigue resistance, resistance to a variety of media, and can maintain high tear strength and elongation at break, good reciprocating bending and fatigue resistance and compression permanent deformation performance in media environments such as esters and ketones. It has excellent anti-corrosion effect when used in diaphragm pumps, is not easy to be damaged, and has a long service life.

[0013] 2. The diaphragm pump diaphragm that is resistant to bending and pressure and the preparation method thereof are achieved by overlapping a pressure-resistant intermediate body, an elastic side body and a wear-resistant surface body in order from the inside to the outside, and a fiber woven mesh fabric is wrapped inside the diaphragm body. The fiber woven mesh fabric is reinforced to greatly improve its pressure resistance and flexural resistance. The combination of the elastic side body and the wear-resistant surface body will further improve the flexural resistance of the diaphragm pump diaphragm, effectively extend the service life of the diaphragm pump diaphragm, and reduce the cost of repair and maintenance of the diaphragm pump. DETAILED DESCRIPTION

[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0015] A bending and pressure-resistant diaphragm pump diaphragm, comprising an elastic side body, a pressure-resistant intermediate body and a wear-resistant surface body; The elastic side body includes the following raw materials in proportion by weight: 80 parts of ternary fluororubber, 8 parts of crosslinking aid, 6 parts of dispersant, 8 parts of accelerator, 10 parts of vulcanizing agent, 53 parts of fiber woven mesh fabric, 9 parts of toughening agent, and 19 parts of elastomer; The pressure-resistant intermediate includes the following raw materials in the following weight proportions: 117 parts of base resin, 60 parts of reinforcement, and 48 parts of support; The wear-resistant surface body comprises the following raw materials in the following weight proportions: 45 parts of base material, 15 parts of surface material, 18 parts of antioxidant and 8 parts of surface modification material.

[0016] The cross-linking auxiliary agent is triallyl isocyanurate, the dispersant is a mixture of urea and glycerol, the antioxidant is antioxidant D, the accelerator is accelerator DM, and the vulcanizing agent is sulfur.

[0017] The elastomer is TPE elastomer particles, and the fiber woven mesh fabric is PET long fiber woven mesh fabric.

[0018] The toughening agent is MBS toughening agent.

[0019] The matrix resin is silicone rubber, and the reinforcement is potassium hexatitanate whisker and aluminum borate whisker.

[0020] The support is a carbon nanotube, and the carbon nanotube is a spiral nanotube.

[0021] The surface modified material is modified nano-TiO2; The surface-modified nano-TiO2 is surface-modified nano-TiO2 prepared by the sol-gel method. 10 ml of butyl titanate is slowly dripped into 35 ml of anhydrous ethanol at room temperature, stirred for 10 minutes and then allowed to stand to form a yellow clear solution. Then 2 ml of glacial acetic acid and 10 ml of anhydrous ethanol are mixed, and vigorously stirred to obtain a transparent solution. Then hydrochloric acid is dripped into the transparent solution to adjust the pH value to 3. In a room temperature water bath, the yellow clear solution is dripped into the transparent solution under vigorous stirring to obtain a light yellow solution. Then, the yellow clear solution is heated in a water bath at 40°C with stirring for 1 hour to obtain a white gel. Subsequently, the gel is dried at 80°C, and then heat-treated at 600°C for 2 hours to obtain white nano-TiO2 powder. Finally, the obtained white nano-TiO2 powder is blended and stirred with sodium dodecyl sulfate for 40 minutes, and the surface-modified nano-TiO2 is obtained after drying.

[0022] Another technical problem to be solved by the present invention is to provide a method for preparing a diaphragm pump diaphragm that is resistant to bending and pressure, comprising the following steps: Step 1: Preparation of elastic side body: Prepare appropriate weight proportions of ternary fluororubber, crosslinking aid, dispersant, accelerator, vulcanizing agent, fiber woven mesh fabric, toughening agent, and elastomer; Step 2: After mixing the ternary fluororubber with the elastomer, toughening agent and dispersant, the mixture is put into an open mill, and a vulcanizing agent is added, and thin-pass refining is performed in the open mill; Step 3: Then the rubber material after the open mixing is placed in a three-roll calendering device for calendering to obtain a film, the distance between the second roll and the third roll is smaller than the distance between the first roll and the second roll, and the film is cut using a slitting machine; Step 4: The fiber woven mesh fabric is then stored, unrolled, flattened, and rolled and laminated with the diaphragm, and the cross-linking aid and accelerator are evenly added. After the lamination, it is introduced into the drying tunnel assembly line, and heated in the drying tunnel assembly line to vulcanize and foam the diaphragm until the diaphragm is completely in a creeping state. The fiber woven mesh fabric is hot-pressed and laminated with the diaphragm layer, flattened, and then punched; Step 5: Preparation of pressure-resistant intermediate: Prepare appropriate weight proportions of matrix resin, reinforcement and support; Step 6: fully mix the matrix resin, reinforcement and support, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step 7: Preparation of wear-resistant surface body: Prepare appropriate weight proportions of base material, fabric, antioxidant and surface modifier; Step 8: fully mix the base material, fabric, antioxidant and surface modification material, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step nine: overlap the prepared pressure-resistant intermediate body, elastic side body and wear-resistant surface body in order from inside to outside, introduce them into the drying tunnel assembly line after compounding, perform hot pressing compounding, flatten, and then punch out. Example

[0023] A bending and pressure-resistant diaphragm pump diaphragm, comprising an elastic side body, a pressure-resistant intermediate body and a wear-resistant surface body; The elastic side body includes the following raw materials in the following weight proportions: 60 parts of ternary fluororubber, 6 parts of crosslinking aid, 1 part of dispersant, 2 parts of accelerator, 5 parts of vulcanizing agent, 40 parts of fiber woven mesh fabric, 6 parts of toughening agent, and 16 parts of elastomer; The pressure-resistant intermediate includes the following raw materials in the following weight proportions: 80 parts of base resin, 30 parts of reinforcement, and 16 parts of support; The wear-resistant surface body comprises the following raw materials in the following weight proportions: 40 parts of base material, 10 parts of surface material, 6 parts of antioxidant and 2 parts of surface modification material.

[0024] The cross-linking auxiliary agent is triallyl isocyanurate, the dispersant is a mixture of urea and glycerol, the antioxidant is antioxidant MB, the accelerator is accelerator DM, and the vulcanizing agent is sulfur.

[0025] The elastomer is TPE elastomer particles, and the fiber woven mesh fabric is PET long fiber woven mesh fabric.

[0026] The toughening agent is MBS toughening agent.

[0027] The matrix resin is silicone rubber and the reinforcement is potassium hexatitanate whisker.

[0028] The support is a carbon nanotube, and the carbon nanotube is a zigzag nanotube.

[0029] The surface modified material is modified nano-TiO2; The surface-modified nano-TiO2 is surface-modified nano-TiO2 prepared by the sol-gel method. 10 ml of butyl titanate is slowly dripped into 35 ml of anhydrous ethanol at room temperature, stirred for 10 minutes and then allowed to stand to form a yellow clear solution. Then 2 ml of glacial acetic acid and 10 ml of anhydrous ethanol are mixed, and vigorously stirred to obtain a transparent solution. Then hydrochloric acid is dripped into the transparent solution to adjust the pH value to 3. In a room temperature water bath, the yellow clear solution is dripped into the transparent solution under vigorous stirring to obtain a light yellow solution. Then, the yellow clear solution is heated in a water bath at 40°C with stirring for 1 hour to obtain a white gel. Subsequently, the gel is dried at 80°C, and then heat-treated at 600°C for 2 hours to obtain white nano-TiO2 powder. Finally, the obtained white nano-TiO2 powder is blended and stirred with sodium dodecyl sulfate for 40 minutes, and the surface-modified nano-TiO2 is obtained after drying.

[0030] Another technical problem to be solved by the present invention is to provide a method for preparing a diaphragm pump diaphragm that is resistant to bending and pressure, comprising the following steps: Step 1: Preparation of elastic side body: Prepare appropriate weight proportions of ternary fluororubber, crosslinking aid, dispersant, accelerator, vulcanizing agent, fiber woven mesh fabric, toughening agent, and elastomer; Step 2: After mixing the ternary fluororubber with the elastomer, toughening agent and dispersant, the mixture is put into an open mill, and a vulcanizing agent is added, and thin-pass refining is performed in the open mill; Step 3: Then the rubber material after the open mixing is placed in a three-roll calendering device for calendering to obtain a film, the distance between the second roll and the third roll is smaller than the distance between the first roll and the second roll, and the film is cut using a slitting machine; Step 4: The fiber woven mesh fabric is then stored, unrolled, flattened, and rolled and laminated with the diaphragm, and the cross-linking aid and accelerator are evenly added. After the lamination, it is introduced into the drying tunnel assembly line, and heated in the drying tunnel assembly line to vulcanize and foam the diaphragm until the diaphragm is completely in a creeping state. The fiber woven mesh fabric is hot-pressed and laminated with the diaphragm layer, flattened, and then punched; Step 5: Preparation of pressure-resistant intermediate: Prepare appropriate weight proportions of matrix resin, reinforcement and support; Step 6: fully mix the matrix resin, reinforcement and support, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step 7: Preparation of wear-resistant surface body: Prepare appropriate weight proportions of base material, fabric, antioxidant and surface modifier; Step 8: fully mix the base material, fabric, antioxidant and surface modification material, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step nine: overlap the prepared pressure-resistant intermediate body, elastic side body and wear-resistant surface body in order from inside to outside, introduce them into the drying tunnel assembly line after compounding, perform hot pressing compounding, flatten, and then punch out.

[0031] The beneficial effects of the present invention are as follows: the preparation method of the diaphragm pump diaphragm that is resistant to bending and pressure makes the diaphragm pump diaphragm have excellent bending and fatigue resistance, resistance to a variety of media, and can maintain high tear strength and tear elongation, good reciprocating bending and fatigue resistance and compression permanent deformation performance in media environments such as esters and ketones. It has excellent anti-corrosion effect when applied to diaphragm pumps, is not easy to be damaged, and has a long service life. The pressure-resistant intermediate body, the elastic side body and the wear-resistant surface body are overlapped in order from the inside to the outside, and a fiber woven mesh fabric is wrapped in the membrane body. The fiber woven mesh fabric is reinforced, and its pressure resistance and flexural resistance are greatly improved. The combination of the elastic side body and the wear-resistant surface body will further improve the flexural resistance of the diaphragm pump diaphragm, effectively extend the service life of the diaphragm pump diaphragm, and reduce the cost of repair and maintenance of the diaphragm pump.

[0032] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A diaphragm pump diaphragm that is resistant to bending and pressure, characterized in that: It includes an elastic side body, a pressure-resistant intermediate body, and a wear-resistant surface body; The elastic side body comprises the following raw materials in proportion by weight: 60-80 parts of ternary fluororubber, 6-8 parts of crosslinking aid, 1-6 parts of dispersant, 2-8 parts of accelerator, 5-10 parts of vulcanizing agent, 40-53 parts of fiber woven mesh fabric, 6-9 parts of toughening agent, and 16-19 parts of elastomer; The pressure-resistant intermediate comprises the following raw materials in the following weight proportions: 80-117 parts of base resin, 30-60 parts of reinforcement, and 16-48 parts of support; The wear-resistant surface body comprises the following raw materials in the following weight proportions: 40-45 parts of base material, 10-15 parts of surface material, 6-18 parts of antioxidant, and 2-8 parts of surface modification material.

2. A bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The cross-linking auxiliary agent is triallyl isocyanurate, the dispersant is a mixture of urea and glycerol, the antioxidant is one of antioxidant MB, antioxidant A, and antioxidant D, the accelerator is one or more of accelerator DM, accelerator D, accelerator M, accelerator TT, and accelerator CE, and the vulcanizing agent is sulfur.

3. A bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The elastomer is TPE elastomer particles, and the fiber woven mesh fabric is PET long fiber woven mesh fabric.

4. A bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The toughening agent is one of an MBS toughening agent and an AK toughening agent.

5. The bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The matrix resin is one of silicone rubber, PERT or HDPE resin powder, and the reinforcement is one of potassium hexatitanate whisker and aluminum borate whisker or a mixture of the two.

6. The bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The support is a carbon nanotube, and the carbon nanotube is at least one of a zigzag nanotube, an armchair nanotube and a spiral nanotube.

7. The bending and pressure-resistant diaphragm pump diaphragm according to claim 1, characterized in that: The surface modification material is modified nano-TiO2; The surface-modified nano-TiO2 is surface-modified nano-TiO2 prepared by a sol-gel method. 10 ml of butyl titanate is slowly dripped into 35 ml of anhydrous ethanol at room temperature, stirred for 10 minutes and then allowed to stand to form a yellow clear solution. Then 2 ml of glacial acetic acid and 10 ml of anhydrous ethanol are mixed, and vigorously stirred to obtain a transparent solution. Then hydrochloric acid is dripped into the solution to adjust the pH value to 3. In a room temperature water bath, the yellow clear solution is dripped into the transparent solution under vigorous stirring to obtain a light yellow solution. Then, the solution is heated in a water bath at 40°C with stirring for 1 hour to obtain a white gel. Then, the gel is dried at 80°C, and then heat-treated at 600°C for 2 hours to obtain a white nano-TiO2 powder. Finally, the obtained white nano-TiO2 powder is blended and stirred with sodium dodecyl sulfate for 40 minutes, and the surface-modified nano-TiO2 is obtained after drying.

8. A method for preparing a bending and pressure-resistant diaphragm pump diaphragm according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Preparation of elastic side body: Prepare appropriate weight proportions of ternary fluororubber, crosslinking aid, dispersant, accelerator, vulcanizing agent, fiber woven mesh fabric, toughening agent, and elastomer; Step 2: After mixing the ternary fluororubber with the elastomer, toughening agent and dispersant, the mixture is put into an open mill, and a vulcanizing agent is added, and thin-pass refining is performed in the open mill; Step 3: Then the rubber material after the open mixing is placed in a three-roll calendering device for calendering to obtain a film, the distance between the second roll and the third roll is smaller than the distance between the first roll and the second roll, and the film is cut using a slitting machine; Step 4: The fiber woven mesh fabric is then stored, unrolled, flattened, and rolled and laminated with the diaphragm, and the cross-linking aid and accelerator are evenly added. After lamination, it is introduced into the drying tunnel assembly line, and heated in the drying tunnel assembly line to vulcanize and foam the diaphragm until the diaphragm is completely in a creeping state. The fiber woven mesh fabric is hot-pressed and laminated with the diaphragm layer, flattened, and then punched; Step 5: Preparation of pressure-resistant intermediate: Prepare appropriate weight proportions of matrix resin, reinforcement and support; Step 6: fully mix the matrix resin, reinforcement and support, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step 7: Preparation of wear-resistant surface body: Prepare appropriate weight proportions of base material, fabric, antioxidant and surface modifier; Step 8: fully mix the base material, fabric, antioxidant and surface modification material, then put them into an open mill for refining, and then take them out for slicing using a slicing machine; Step nine: overlap the prepared pressure-resistant intermediate body, elastic side body and wear-resistant surface body in order from inside to outside, introduce them into the drying tunnel assembly line after compounding, perform hot pressing compounding, flatten, and then punch out.

Citation Information

Patent Citations

  • Diaphragm of hydraulic diaphragm pump and production technology of diaphragm

    CN107828159A

  • Fluorine rubber with high elongation at rupture and excellent flex fatigue resistance and preparation method of flex fatigue resistant fluorine rubber

    CN109265878A

  • Deflection-resistant liquid-medicine-resistant diaphragm pump diaphragm and preparation method thereof

    CN116814022A

  • Compound environmental protection diaphragm of diaphragm pump

    CN205225649U