Degradable multi-layer high-barrier film as well as preparation method and application thereof
The multi-layer structure is designed through the co-extrusion process, using a blend of polyterephthalic acid/butylene adipate and inorganic filler as the outer layer, polyterephthalic acid/butylene adipate and glutamate and The blend of adhesive resin is used as the adhesive layer and pure polyglycolic acid is used as the barrier layer, which solves the problems of poor processing performance and insufficient adhesion of multilayer films in the prior art, and achieves high barrier, degradability and high Tough multi-layer film preparation.
Patent Information
- Application Number
- CN202310606410.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-26
AI Technical Summary
The prior art has problems such as poor processing performance, insufficient adhesion and low process efficiency when preparing high barrier multilayer films, especially poor adhesion between pure PGA layers and other layer structures and adhesive rollers at high processing temperatures. .
The multi-layer structure is designed using co-extrusion process. The outer layer is a blend of polyterephthalic acid/butylene adipate and inorganic filler, and the adhesive layer is polyterephthalic acid/butylene adipate. The blend of ester and tackifying resin, and the barrier layer is pure polyglycolic acid, a high barrier film with good processing performance, non-layered and biodegradable high barrier film is prepared through multi-layer coextrusion technology.
The high barrier properties of multi-layer films are achieved, process performance and adhesion are improved, and the full biodegradability is maintained, and the problems of poor adhesion and adhesive rollers are solved, which improves the overall toughness and processing efficiency of the film.
Smart Images

Figure BDA0004250709230000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of multilayer films, and in particular relates to a degradable multilayer high-barrier film and a preparation method and application thereof. Background Art
[0002] Polyglycolic acid (PGA) has a glass transition temperature (Tg) of 35°C to 45°C and a peak melting temperature (Tg) of 220°C to 233°C. m ) is a semi-crystalline aliphatic polyester with excellent mechanical properties, especially the highest elastic modulus of 6-7GPa, which is essential for providing substantial support for load-bearing applications. In addition, PGA has excellent gas barrier properties and is basically unaffected by ambient temperature. Therefore, placing PGA in the core layer as a barrier layer is an ideal material choice for multi-layer barrier films. In addition, PGA can be rapidly degraded and eventually decomposed into water and carbon dioxide. It is a material recognized by the world to protect the earth's environment and life. Therefore, the development of fully degradable multi-layer barrier films based on PGA can solve the problem that traditional composite barrier films are difficult to recycle. However, PGA has high processing temperatures, poor toughness, and poor adhesion to other resins, so its application in high barrier films is greatly limited.
[0003] Patent document CN113388136A discloses a PGA-reinforced biodegradable film, the raw materials of which include, by weight: 100 parts of biodegradable polyester, 10-30 parts of polyglycolic acid PGA, 20-30 parts of bio-based filler, 0.2-1 parts of chain extender, and 5-15 parts of plasticizer; the processing method of this patent is to first obtain a composite material masterbatch by melt extrusion and then use a blow molding machine to blow-mold the obtained composite material masterbatch, and a multilayer film cannot be obtained.
[0004] Patent document CN109566210A discloses a multi-layer composite multifunctional fully biodegradable plastic ground film, which includes at least one ground-contacting layer and one supporting layer; the ground-contacting layer contains the following components by mass: 100 parts of fully biodegradable polyester, 5-10 parts of reinforcing agent, 0-30 parts of filler, 5-20 parts of ground-contacting modified masterbatch, and 0-5 parts of chain extender; the supporting layer contains the following components by mass: 100 parts of fully biodegradable polyester, 5-10 parts of reinforcing agent, 0-30 parts of filler, 0-8 parts of auxiliary agent masterbatch, and 0-5 parts of chain extender. There is no pure PGA layer in the multi-layer film of this patent, and the improvement of barrier properties is affected.
[0005] Patent document CN113232395A discloses a fully biodegradable composite film material with barrier properties and its packaging bag. The composite film material includes a cellulose layer, a PGA layer, a PBAT layer, a first adhesive layer sandwiched between the PBAT layer and the PGA layer, and a second adhesive layer between the PGA layer and the cellulose layer from top to bottom. The PBAT layer, the first adhesive layer, the PGA layer, the second adhesive layer and the cellulose layer are combined together through a composite film forming technology. The patent combines a cellulose layer with printing adaptability but poor extensibility and no heat sealability with a PGA with barrier properties through a second adhesive layer, and then combines it with a PBAT layer with heat sealability and extensibility through a first adhesive layer. The properties of the two are complementary, and a composite film material with good surface wetting tension, heat resistance and heat sealability, adaptability to low-temperature freezing, and certain barrier properties can be made. Most of the materials are derived from degradable raw materials, which is green and environmentally friendly. However, this patent uses a hot pressing molding process, which is complex and inefficient.
[0006] In view of this, continuing to develop multilayer films with high barrier properties and their preparation methods has become a direction worthy of research. Summary of the invention
[0007] The purpose of the present invention is to provide a degradable multilayer high barrier film and its preparation method and application in view of the shortcomings of the prior art in preparing high barrier multilayer films. The co-extrusion process is adopted, and the barrier layer in the multilayer film is pure polyglycolic acid. By designing the multilayer structure and improving the materials of each layer, a multilayer film with good processing performance, no stratification, full biodegradability and high barrier properties can be obtained.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] In a first aspect, a degradable multilayer high barrier film is provided, the multilayer high barrier film comprising: an outer layer / adhesive layer / barrier layer / adhesive layer / outer layer arranged in sequence; wherein,
[0010] The outer layer is a blend I of polybutylene terephthalate / adipate and an inorganic filler;
[0011] The adhesive layer is a blend II of polybutylene terephthalate / adipate and a tackifying resin;
[0012] The barrier layer is polyglycolic acid.
[0013] According to the multilayer high barrier film provided by the present invention, in one embodiment, the thickness of the multilayer high barrier film is 50-300 μm (for example, 55 μm, 60 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm).
[0014] In one embodiment, the thickness ratio of each layer in the multi-layer high barrier film is outer layer: adhesive layer: barrier layer = 2:2:1 to 1:1:2, for example, 2:2:1.4, 2:2:2, 2:2:2.5, 2:2:3, 2:2:3.6.
[0015] According to the multilayer high barrier film provided by the present invention, in some embodiments, in the blend I of polybutylene terephthalate / adipate and an inorganic filler, based on the total weight of the blend I, the content of polybutylene terephthalate / adipate is 60wt% to 95wt% (for example, 65wt%, 70wt%, 75wt%, 80wt%, 90wt%), and the content of the inorganic filler is 5wt% to 40wt% (for example, 6wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%).
[0016] In some embodiments, the inorganic filler is selected from one or more of SiO2, calcium carbonate, montmorillonite and talc.
[0017] According to the multilayer high barrier film provided by the present invention, in some embodiments, in the blend II of polybutylene terephthalate / adipate and tackifying resin, based on the total weight of the blend II, the content of polybutylene terephthalate / adipate is 80wt% to 95wt% (for example, 82wt%, 85wt%, 88wt%, 90wt%, 93wt%), and the content of the tackifying resin is 5wt% to 20wt% (for example, 6wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt%).
[0018] In some embodiments, the tackifying resin is a natural series resin.
[0019] In some embodiments, the natural series resin is selected from one or more of rosin, rosin derivatives and terpene resins.
[0020] In some embodiments, the rosin is selected from gum rosin, tall oil rosin, wood rosin;
[0021] In some embodiments, the rosin derivative is selected from hydrogenated rosin, disproportionated rosin, polymerized rosin, esterified rosin, and maleated rosin;
[0022] In some embodiments, the terpene resin is selected from α-terpene resin, β-terpene resin, and terpene phenolic resin.
[0023] According to the multilayer high barrier film provided by the present invention, in some embodiments, the weight average molecular weight of the polyglycolic acid is 100,000 to 300,000 (for example, 120,000, 150,000, 200,000, 250,000), and the melt index is 5.0 to 80 g / 10 min (for example, 6.0 g / 10 min, 10.0 g / 10 min, 15 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 50 g / 10 min, 60 g / 10 min, 70 g / 10 min).
[0024] In a second aspect, a method for preparing the multilayer high barrier film as described above is provided, comprising the following steps:
[0025] 1) drying polybutylene terephthalate / adipate and inorganic filler (e.g. in a vacuum drying oven), preferably, the drying process conditions include: a time of 2-4 hours (e.g., 2.5 hours, 3 hours) and a temperature of 30-50° C. (e.g., 35° C., 40° C., 45° C.);
[0026] Weighing the dried polybutylene terephthalate / adipate and inorganic filler, blending them, and melt-extruding and granulating them through a twin-screw extruder to obtain an outer layer resin material;
[0027] 2) drying the polybutylene terephthalate / adipate and the tackifying resin (e.g. in a vacuum drying oven), preferably, the drying process conditions include: a time of 2-4 hours (e.g., 2.5 hours, 3 hours) and a temperature of 30-50° C. (e.g., 35° C., 40° C., 45° C.);
[0028] Weighing the dried polybutylene terephthalate / adipate and tackifying resin, blending them, and melt-extruding and granulating them through a twin-screw extruder to obtain an adhesive layer resin material;
[0029] 3) The outer layer resin material, the adhesive layer resin material and the polyglycolic acid are co-extruded in multiple layers, and subjected to a casting or blown film process to obtain the degradable multi-layer high barrier film.
[0030] According to the preparation method of the present invention, in some embodiments, the adhesion of the multilayer high barrier film is greater than 1N / cm (for example, 1.5N / cm, 2N / cm, 4N / cm, 8N / cm, 10N / cm), and the water vapor transmission rate is ≤10g / (m 2 ·day), for example, 9g / (m 2 ·day)、5g / (m 2 ·day)、2g / (m 2 ·day)、1g / (m 2 ·day)、0.5g / (m2 ·day)、0.1g / (m 2 ·day)、0.05g / (m 2 ·day)、0.01g / (m 2 ·day), oxygen permeability ≤3cm 3 / (m 2 ·day·0.1MPa), for example, 2.5cm 3 / (m 2 ·day·0.1MPa)、2cm 3 / (m 2 ·day·0.1MPa)、1.5cm 3 / (m 2 ·day·0.1MPa)、1.0cm 3 / (m 2 ·day·0.1MPa)、0.5cm 3 / (m 2 ·day·0.1MPa)、0.1cm 3 / (m 2 ·day·0.1MPa)、0.05cm 3 / (m 2 ·day·0.1MPa)、0.01cm 3 / (m 2 ·day·0.1MPa).
[0031] According to the preparation method of the present invention, in some embodiments, the melt extrusion process conditions described in step 1) include: the temperature of the conveying section of the extruder is 130-160°C (e.g., 140°C, 150°C), the temperature of the melting section is 160-190°C (e.g., 170°C, 180°C), the temperature of the mixing section is 170-200°C (e.g., 180°C, 190°C), the temperature of the exhaust section is 160-190°C (e.g., 170°C, 180°C), the temperature of the homogenizing section is 150-180°C (e.g., 160°C, 170°C); the screw speed is 50-200rpm (e.g., 60rpm, 100rpm, 150rpm).
[0032] In some embodiments, the melt extrusion process conditions described in step 2) include: the temperature of the conveying section of the extruder is 130-160°C (e.g., 140°C, 150°C), the temperature of the melting section is 160-190°C (e.g., 170°C, 180°C), the temperature of the mixing section is 170-200°C (e.g., 180°C, 190°C), the temperature of the exhaust section is 160-190°C (e.g., 170°C, 180°C), the temperature of the homogenizing section is 140-170°C (e.g., 150°C, 160°C); the screw speed is 50-200rpm (e.g., 60rpm, 100rpm, 150rpm).
[0033] In some embodiments, the process conditions of the multi-layer co-extrusion in step 3) include:
[0034] The extrusion temperature of the outer layer is 180-220°C (e.g., 185°C, 190°C, 200°C, 210°C); the extrusion temperature of the adhesive layer is 180-220°C (e.g., 185°C, 190°C, 200°C, 210°C); the extrusion temperature of the barrier layer is 230-260°C (e.g., 235°C, 240°C, 250°C, 255°C); the die head temperature is 240-260°C (e.g., 235°C, 240°C, 250°C, 255°C).
[0035] In a third aspect, there is provided a multilayer high barrier film as described above or a multilayer high barrier film prepared by the preparation method as described above, for use in the packaging field, especially in food, electronics, and drug packaging.
[0036] In the present invention, the outer layer is a blend of polybutylene terephthalate / adipate and an inorganic filler, which can increase the crystallization temperature, crystallize faster, and effectively solve the roller sticking problem.
[0037] Although PGA has good barrier properties and is an ideal material for improving the barrier properties of multilayer films, when pure PGA is used as a barrier layer in a multilayer film, there is often a problem of poor adhesion between pure PGA and other layer structures (such as PBAT), which is one of the technical obstacles to be solved by the present invention. In addition, PGA has a very high melting point, and the processing temperature difference with other tough biodegradable plastics in the multilayer film is relatively large, which will lead to poor co-extrusion processing performance. At the high processing temperature of PGA, other biodegradable resins are difficult to cool and crystallize, and the problem of sticking to the roller will occur. This is also one of the problems to be solved in this application when pure PGA is used as the core layer to prepare a multilayer high barrier film.
[0038] Moreover, PGA has poor toughness, so an outer layer with high toughness needs to be selected as a protective layer to improve the overall toughness of the film; and in order to maintain full biodegradability, the selection of the type of applicable outer layer material is critical.
[0039] Compared with the prior art, the present invention designs a multilayer structure, and the outer layer uses a blend of PBAT and inorganic fillers, which can improve the sticking and rolling problem of the multilayer film caused by the outer layer material at high processing temperature, improve the overall toughness of the multilayer film, and maintain full biodegradability; and the adhesive layer uses a blend of PBAT and a tackifying resin, which can improve the adhesion between PBAT and PGA; while improving the processing performance and the adhesion between pure PGA and other layer structures, the barrier layer uses pure PGA, which can maintain the high barrier performance of the multilayer film. The present invention uses a multi-layer co-extrusion technology to prepare a high-barrier multilayer film with good processing performance, no stratification, and full biodegradability. DETAILED DESCRIPTION
[0040] In order to understand the technical features and contents of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described here.
[0041] <Source of raw materials>
[0042] Polyglycolic acid, weight average molecular weight of 130,000, melt index of 26 g / 10 min (240 ° C, 2.16 kg), purchased from Shanghai Pujing Chemical Technology Co., Ltd.;
[0043] Polybutylene adipate terephthalate (PBAT), BASF C1200, purchased from BASF;
[0044] Talc (powder), 2500 mesh, purchased from Changzhou Rongao Chemical New Materials Co., Ltd.;
[0045] Tackifying resin, terpene resin, purchased from Changzhou Jiatong Chemical Co., Ltd.;
[0046] Other raw materials used in the examples and comparative examples are commonly available commercially and will not be described in detail here.
[0047] Example 1
[0048] The method for preparing a degradable multi-layer high barrier film comprises the following steps:
[0049] (1) Preparation of outer layer resin A1: Dry the PBAT and talc to be used in a vacuum drying oven at 50° C. for 4 hours; weigh 1000 g of the dried PBAT and 300 g of talc, melt extrude and granulate in a twin-screw extruder to obtain outer layer resin A1, wherein:
[0050] The conditions for melt extrusion were as follows: the temperature of the conveying section was 150°C, the temperature of the melting section was 190°C, the temperature of the mixing section was 190°C, the temperature of the exhaust section was 190°C, the temperature of the homogenizing section was 170°C, and the screw speed was 100 rpm;
[0051] (2) Preparation of adhesive layer resin B1: 950 g of dried PBAT and 50 g of terpene resin were weighed and melt-extruded and granulated in a twin-screw extruder to obtain adhesive layer resin B1, wherein:
[0052] The conditions for melt extrusion were as follows: the temperature of the conveying section was 150°C, the temperature of the melting section was 190°C, the temperature of the mixing section was 190°C, the temperature of the exhaust section was 190°C, the temperature of the homogenizing section was 170°C, and the screw speed was 100 rpm;
[0053] (3) Multi-layer co-extrusion: Add polyglycolic acid to the inner layer hopper, add the prepared resin B1 to the core layer hopper, add the prepared resin A1 to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 190-210°C, and 190-210°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up. The die head temperature is 240-260°C and the roller temperature is 10-40°C. A degradable multi-layer high barrier film is obtained.
[0054] The thickness of the prepared multilayer high barrier film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0055] Example 2
[0056] The method for preparing a degradable multi-layer high barrier film comprises the following steps:
[0057] (1) Preparation of outer layer resin A1: the same as in Example 1;
[0058] (2) Preparation of adhesive layer resin B2: 900 g of dried PBAT and 100 g of terpene resin were weighed and melt-extruded and granulated in a twin-screw extruder to obtain adhesive layer resin B2, wherein:
[0059] The conditions for melt extrusion were as follows: the temperature of the conveying section was 150°C, the temperature of the melting section was 190°C, the temperature of the mixing section was 190°C, the temperature of the exhaust section was 190°C, the temperature of the homogenizing section was 170°C, and the screw speed was 100 rpm;
[0060] (3) Multi-layer co-extrusion: Add polyglycolic acid to the inner layer hopper, add the prepared resin B2 to the core layer hopper, and add the prepared resin A1 to the outer layer hopper. Co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 190-210°C, and 190-210°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up. The die head temperature is 240-260°C and the roller temperature is 10-40°C. A degradable multi-layer high barrier film is obtained.
[0061] The thickness of the prepared multilayer high barrier film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0062] Example 3
[0063] The method for preparing a degradable multi-layer high barrier film comprises the following steps:
[0064] (1) Preparation of outer layer resin A2: Dry the PBAT and SiO2 to be used in a vacuum drying oven at 50° C. for 4 hours; weigh 1000 g of the dried PBAT and 200 g of SiO2, melt extrude and granulate them in a twin-screw extruder to obtain outer layer resin A2; wherein,
[0065] The conditions for melt extrusion were as follows: the temperature of the conveying section was 150°C, the temperature of the melting section was 190°C, the temperature of the mixing section was 190°C, the temperature of the exhaust section was 190°C, the temperature of the homogenizing section was 170°C, and the screw speed was 100 rpm;
[0066] (2) Preparation of adhesive layer resin B1: the same as in Example 1;
[0067] (3) Multilayer coextrusion: The process conditions and non-operation steps refer to step (3) of Example 1.
[0068] The thickness of the prepared multilayer high barrier film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0069] Example 4
[0070] The method for preparing a degradable multi-layer high barrier film comprises the following steps:
[0071] (1) Preparation of outer layer resin A3: Referring to Example 1, except that 1000 g of dried PBAT and 60 g of talc were weighed and melt-extruded and granulated in a twin-screw extruder to obtain outer layer resin A3;
[0072] (2) Preparation of adhesive layer resin B2: the same as in Example 2;
[0073] (3) Multi-layer co-extrusion: Add polyglycolic acid to the inner layer hopper, add the prepared resin B2 to the core layer hopper, add the prepared resin A3 to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 190-210°C, and 190-210°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up. The die head temperature is 240-260°C and the roller temperature is 10-40°C. A degradable multi-layer high barrier film is obtained.
[0074] The thickness of the prepared multilayer high barrier film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0075] Comparative Example 1
[0076] The method for preparing a multilayer film comprises the following steps:
[0077] Add polyglycolic acid to the inner layer hopper, add PBAT to the core layer hopper, add PBAT to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260° C., 190-210° C., and 190-210° C. respectively). The outer, middle, and inner five layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 240-260° C., and the roller temperature is 10-40° C.; thus, a multi-layer film is obtained.
[0078] The thickness of the prepared multilayer film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0079] Comparative Example 2
[0080] The method for preparing a multilayer film comprises the following steps:
[0081] PBAT is added to the inner layer hopper, PBAT is added to the core layer hopper, and PBAT is added to the outer layer hopper. The three screw extruders (the working temperatures of the inner layer, the core layer, and the outer layer are 190-210° C., 190-210° C., and 190-210° C., respectively) are used for co-extrusion. The outer, middle, and inner five layers are co-extruded and cast into a film through a die head, and then rolled up. The die head temperature is 190-210° C., and the roller temperature is 10-40° C.
[0082] The thickness of the prepared multilayer film is 100 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0083] The multilayer film structure obtained in the above embodiments and comparative examples can be schematically represented as: A / B / C / B / A.
[0084] Test method:
[0085] (1) Melt index: measured according to GB / T 3682-2000;
[0086] (2) Water vapor transmission rate: measured according to GB / T 30412-2013 method;
[0087] (3) Oxygen transmission rate: measured according to GB / T 1038-2000;
[0088] (4) Peel strength test, measured according to GBT2792-2014 method;
[0089] (5) Processability testing and judgment criteria: The processability of excellent, good, and poor means that the processability is excellent if it does not stick to the roller and can be produced continuously; it is good if it sticks to the roller slightly and can be produced continuously; and it is poor if it sticks to the roller and cannot be produced continuously.
[0090] Table 1 Performance test results of the multilayer films prepared in various embodiments and comparative examples
[0091]
[0092] It can be seen from the test results in Table 1 that: by comparing Examples 1-4 with Comparative Example 2, the barrier properties of the multilayer film can be significantly improved by using composite PGA as a barrier layer; by comparing Examples 1-4 with Comparative Example 1, the bonding problem of the multilayer barrier film and the processability of the multilayer film can be improved by selecting a suitable component as the adhesive layer and a suitable component as the outer layer in the multilayer film; it can be seen from Examples 1-4 that the peel strength and processability of the multilayer film can be adjusted by changing the content of the tackifying resin and the type and content of the inorganic filler.
[0093] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A degradable multi-layer high barrier film, characterized in that: The multi-layer high barrier film comprises: an outer layer / adhesive layer / barrier layer / adhesive layer / outer layer arranged in sequence; wherein, The outer layer is a blend I of polybutylene terephthalate / adipate and an inorganic filler; The adhesive layer is a blend II of polybutylene terephthalate / adipate and a tackifying resin; The barrier layer is polyglycolic acid; Preferably, the thickness of the multilayer high barrier film is 50-300 μm; Preferably, the thickness ratio of each layer in the multi-layer high barrier film is outer layer: adhesive layer: barrier layer = 2:2:1 to 1:1:
2.
2. The multi-layer high barrier film according to claim 1, characterized in that: In the blend I of polybutylene terephthalate / adipate and an inorganic filler, based on the total weight of the blend I, the content of polybutylene terephthalate / adipate is 60 wt % to 95 wt %, and the content of the inorganic filler is 5 wt % to 40 wt %.
3. The multi-layer high barrier film according to claim 1, characterized in that: The inorganic filler is selected from one or more of SiO2, calcium carbonate, montmorillonite and talc.
4. The multi-layer high barrier film according to claim 1, characterized in that: In the blend II of polybutylene terephthalate / adipate and tackifying resin, based on the total weight of the blend II, the content of polybutylene terephthalate / adipate is 80 wt % to 95 wt %, and the content of the tackifying resin is 5 wt % to 20 wt %.
5. The multi-layer high barrier film according to claim 1, characterized in that: The tackifying resin is a natural series resin; Preferably, the natural series resin is selected from one or more of rosin, rosin derivatives and terpene resins.
6. The multi-layer high barrier film according to claim 1, characterized in that: The weight average molecular weight of the polyglycolic acid is 100,000 to 300,000, and the melt index is 5.0 to 80 g / 10 min.
7. The method for preparing a multilayer high barrier film according to any one of claims 1 to 6, characterized in that: The steps include: 1) drying polybutylene terephthalate / adipate and inorganic filler; Weighing the dried polybutylene terephthalate / adipate and inorganic filler, blending them, and melt-extruding and granulating them through a twin-screw extruder to obtain an outer layer resin material; 2) drying polybutylene terephthalate / adipate and tackifying resin; Weighing the dried polybutylene terephthalate / adipate and tackifying resin, blending them, and melt-extruding and granulating them through a twin-screw extruder to obtain an adhesive layer resin material; 3) co-extruding the outer layer resin material, the adhesive layer resin material and the polyglycolic acid in multiple layers, and subjecting the co-extrusion to a casting or blown film process to obtain the degradable multi-layer high barrier film; Preferably, the multi-layer high barrier film has an adhesive force of >1N / cm and a water vapor transmission rate of ≤10g / (m 2 ·day), oxygen permeability ≤3cm 3 / (m 2 ·day·0.1MPa).
8. The preparation method according to claim 7, characterized in that: The melt extrusion process conditions described in step 1) include: the temperature of the conveying section of the extruder is 130-160°C, the temperature of the melting section is 160-190°C, the temperature of the mixing section is 170-200°C, the temperature of the exhaust section is 160-190°C, the temperature of the homogenization section is 150-180°C; the screw speed is 50-200rpm; and / or The melt extrusion process conditions described in step 2) include: the temperature of the conveying section of the extruder is 130-160°C, the temperature of the melting section is 160-190°C, the temperature of the mixing section is 170-200°C, the temperature of the exhaust section is 160-190°C, the temperature of the homogenizing section is 140-170°C; the screw speed is 50-200rpm.
9. The preparation method according to claim 7, characterized in that: The process conditions of multi-layer coextrusion in step 3) include: The extrusion temperature of the outer layer is 180-220°C; the extrusion temperature of the adhesive layer is 180-220°C; the extrusion temperature of the barrier layer is 230-260°C; and the die head temperature is 240-260°C.
10. Use of the multilayer high barrier film according to any one of claims 1 to 6 or the multilayer high barrier film prepared by the preparation method according to any one of claims 7 to 9 in the packaging field, especially in food, electronics and drug packaging.
Citation Information
Patent Citations
Multi-layer composite multifunctional fully biologically degradable plastic mulching film and preparation method thereof
CN109566210A
Full-biodegradable composite film material with barrier property and packaging bag
CN113232395A
PGA-enhanced degradable film and preparation method thereof
CN113388136A
Composite material for poly(butylene succinate) degradable film and preparation method thereof
CN103013065A
Biodegradation express delivery packaging bag and preparation technology thereof
CN105416797A