Preparation method of gold nano circular ring array
By replacing electron beam lithography with photolithography, the deposition and etching technology of photoresist, alumina film and gold film was used to solve the problems of complex operation, high cost and low efficiency in the preparation of gold nanoring arrays, and realize the Efficient and low-cost mass production.
Patent Information
- Application Number
- CN202411131860.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing gold nanoring array preparation methods rely on electron beam lithography, which are complex in operation, high in cost and low in efficiency, making it difficult to achieve large-scale mass production.
Instead of electron beam lithography, a circular hole array is formed by applying photoresist to the upper surface of the substrate, exposure and development are carried out, and alumina films and gold-plated films are deposited, and vertical etching and wet corrosion are carried out. Form a gold nanoring array.
It realizes simple operation, low production cost and high preparation efficiency, and can prepare large-scale mass-produced gold nanoring arrays, and flexibly adjusts the size of the nanorings by adjusting the thickness of the alumina film and gold film.
Smart Images

Figure CN119018844A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gold nanomaterial preparation, and particularly relates to a method for preparing a gold nano ring array. Background Art
[0002] Nanoscale precious metal (gold, silver, platinum, etc.) particles have a strong electric field-magnetic field coupling effect, which makes them widely used in micro-nano gratings, magnetic storage, biosensors and photoelectric catalysis. This electric field-magnetic field coupling effect is caused by the localized surface plasma resonance (LSPR) effect between metal nanoparticles and incident light. The strength of the LSPR effect is often closely related to the material, morphology, size and arrangement of the particles. Therefore, technicians in this field have prepared nanoarrays of various morphologies, such as spherical, disc-shaped, cylindrical and hemispherical, etc., to prepare devices with different optical properties. Compared with the above-mentioned gold nanoarrays of several traditional morphologies, the gold nanoring array can comprehensively adjust the inner diameter, ring thickness and height to meet the use requirements of the resulting device, and has a wider research and application value.
[0003] Currently, gold nanoring arrays are mainly manufactured by electron beam lithography (EBL). However, the EBL method is very complicated to operate, has high production costs, and has very low preparation efficiency, making it difficult to mass produce. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a gold nanoring array. The preparation method provided by the present invention is simple to operate, has low production cost, high preparation efficiency, and can be mass-produced.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a gold nanoring array, comprising the following steps:
[0007] Applying photoresist on the upper surface of the substrate to form a photoresist mask layer; sequentially exposing and developing the photoresist mask layer to form a circular hole array in the photoresist mask layer, thereby obtaining a photoresist developed substrate; the circular hole array is formed by a plurality of circular holes that are not in contact with each other, the bottom surface of each circular hole exposes the substrate, and the photoresist mask layer is retained outside the circular hole;
[0008] An aluminum oxide film is prepared on the upper surface of the photoresist development substrate by atomic layer deposition, the remaining photoresist mask layer and the aluminum oxide film on the upper surface of the photoresist mask layer are removed, and the remaining aluminum oxide film in each circular hole is retained as an aluminum oxide column, and an aluminum oxide column array formed by the aluminum oxide columns is obtained on the upper surface of the substrate, and the substrate is exposed between adjacent aluminum oxide columns;
[0009] A gold film is prepared on the top and side wall of the alumina cylinder and the exposed upper surface of the substrate between adjacent alumina cylinders by electron beam evaporation to obtain a gold-plated substrate;
[0010] The gold film on the top of each alumina cylinder and the upper surface of the substrate between adjacent alumina cylinders on the gold-plated substrate is removed by vertical etching, and the remaining gold film on the side wall of the alumina cylinder is retained;
[0011] The aluminum oxide column array is removed by wet etching to obtain a gold nano-ring array formed by the remaining gold film on the upper surface of the substrate.
[0012] Preferably, the substrate includes a glass substrate, a silicon substrate, a gallium nitride substrate, a silicon carbide substrate or a gallium oxide substrate.
[0013] Preferably, the thickness of the photoresist mask layer is 550-650 nm; and the rotation rate of the carrier used during the coating is 3000-3200 rpm.
[0014] Preferably, the intensity of the light used for exposure is 2.0-2.1 mW / cm 2 The exposure time is 10 to 12 seconds, and the development time is 30 to 35 seconds.
[0015] Preferably, the circular holes have a diameter of 375-425 nm, a period of 580-620 nm, and a depth of 600-605 nm.
[0016] Preferably, the thickness of the aluminum oxide film is 390-410 nm, and the coating rate of the aluminum oxide film is
[0017]
[0018] Preferably, the thickness of the gold film is 38-42 nm, and the evaporation rate of the gold film is
[0019] Preferably, the conditions for the vertical etching include: the angle of the stage is 0°, the flow rate of argon gas is 8-10 sccm; and the time for the vertical etching is 12-18 min.
[0020] Preferably, the reagent used for the wet etching is a phosphoric acid aqueous solution, and the mass fraction of the phosphoric acid aqueous solution is 2-4%; the temperature of the wet etching is 70-75°C.
[0021] Preferably, the step of coating the photoresist on the upper surface of the substrate includes sequentially subjecting the substrate to an acid treatment and an alkali treatment;
[0022] The reagents used for the acid treatment are concentrated sulfuric acid and hydrogen peroxide, the concentration of the concentrated sulfuric acid is 98wt%, the concentration of the hydrogen peroxide is 30wt%-35wt%, and the volume ratio of the concentrated sulfuric acid to the hydrogen peroxide is 1-3:1-2; the time of the acid treatment is 10-20min;
[0023] The reagents used for the alkali treatment are ammonia water and hydrogen peroxide. The concentration of the ammonia water is 0.8-0.9 g / mL, the concentration of the hydrogen peroxide is 30wt%-35wt%, and the volume ratio of the ammonia water to the hydrogen peroxide is 1-3:1-2. The time of the alkali treatment is 10-15 minutes.
[0024] The invention provides a method for preparing a gold nano-ring array, which comprises the following steps: coating a photoresist on the upper surface of a substrate to form a photoresist mask layer; sequentially exposing and developing the photoresist mask layer to form a circular hole array in the photoresist mask layer to obtain a photoresist development substrate; the circular hole array is formed by a plurality of circular holes that are not in contact with each other, the bottom surface of each circular hole exposes the substrate, and the photoresist mask layer is retained outside the circular hole; preparing an aluminum oxide film on the upper surface of the photoresist development substrate in an atomic layer deposition manner, removing the remaining photoresist mask layer and the aluminum oxide film on the upper surface of the photoresist mask layer, and retaining each circular hole; The aluminum oxide film in the hole is used as an aluminum oxide cylinder, and an aluminum oxide cylinder array formed by aluminum oxide cylinders is obtained on the upper surface of the substrate, and the substrate is exposed between adjacent aluminum oxide cylinders; a gold film is prepared on the top and side wall of the aluminum oxide cylinder and the upper surface of the substrate exposed between adjacent aluminum oxide cylinders by electron beam evaporation to obtain a gold-plated substrate; the gold film on the top of each aluminum oxide cylinder on the gold-plated substrate and the upper surface of the substrate between adjacent aluminum oxide cylinders is removed by vertical etching, and the remaining gold film on the side wall of the aluminum oxide cylinder is retained; the aluminum oxide cylinder array is removed by wet etching, and a gold nano-ring array formed by the remaining gold film is obtained on the upper surface of the substrate. The present invention replaces electron beam lithography with photolithography, is simple to operate, has higher lithography efficiency and lower production cost than traditional electron beam lithography methods, and can be mass-produced.
[0025] Furthermore, the present invention can flexibly adjust the size of the obtained gold nanorings by the height of the deposited aluminum oxide film and the thickness of the gold film, and has strong operability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0027] Figure 1 is a cross-sectional view of a photoresist glass substrate and a photoresist developing glass substrate;
[0028] Figure 2 It is a cross-sectional view of an aluminum oxide film-coated substrate and a glass substrate after debonding;
[0029] Figure 3 is a cross-sectional view of a gold-plated glass substrate and a glass substrate after vertical etching;
[0030] Figure 4 It is a top view of the gold nanoring array;
[0031] Among them, 1-glass substrate; 2-photoresist mask layer; 3-aluminum oxide film; 4-gold film. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing a gold nanoring array, comprising the following steps:
[0033] Applying photoresist on the upper surface of the substrate to form a photoresist mask layer; sequentially exposing and developing the photoresist mask layer to form a circular hole array in the photoresist mask layer, thereby obtaining a photoresist developed substrate; the circular hole array is formed by a plurality of circular holes that are not in contact with each other, the bottom surface of each circular hole exposes the substrate, and the photoresist mask layer is retained outside the circular hole;
[0034] An aluminum oxide film is prepared on the upper surface of the photoresist development substrate by atomic layer deposition, the remaining photoresist mask layer and the aluminum oxide film on the upper surface of the photoresist mask layer are removed, and the remaining aluminum oxide film in each circular hole is retained as an aluminum oxide column, and an aluminum oxide column array formed by the aluminum oxide columns is obtained on the upper surface of the substrate, and the substrate is exposed between adjacent aluminum oxide columns;
[0035] A gold film is prepared on the top and side wall of the alumina cylinder and the exposed upper surface of the substrate between adjacent alumina cylinders by electron beam evaporation to obtain a gold-plated substrate;
[0036] The gold film on the top of each alumina cylinder and the upper surface of the substrate between adjacent alumina cylinders on the gold-plated substrate is removed by vertical etching, and the remaining gold film on the side wall of the alumina cylinder is retained;
[0037] The aluminum oxide column array is removed by wet etching to obtain a gold nano-ring array formed by the remaining gold film on the upper surface of the substrate.
[0038] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0039] In the present invention, the substrate preferably includes a glass substrate, a silicon substrate, a gallium nitride substrate, a silicon carbide substrate or a gallium oxide substrate, and more preferably a glass substrate or a silicon carbide substrate. The substrate used in the embodiment of the present invention is a glass substrate, and the glass substrate is a 4-inch glass wafer.
[0040] In the present invention, the method of coating the photoresist on the upper surface of the substrate preferably includes sequentially subjecting the substrate to an acid treatment and an alkali treatment. The reagents used for the acid treatment of the present invention are preferably concentrated sulfuric acid and hydrogen peroxide; the concentration of the concentrated sulfuric acid is preferably 98wt%; the concentration of the hydrogen peroxide is preferably 30-35wt%, specifically 30wt%, 32wt% or 35wt%; the volume ratio of the concentrated sulfuric acid to the hydrogen peroxide is preferably 1-3:1-2, more preferably 2:1. The acid treatment of the present invention is preferably carried out under ultrasonic conditions; the time of the acid treatment is preferably 10-20min, more preferably 15min. The present invention removes organic matter and metal particle impurities remaining on the surface of the substrate by acid treatment. The reagents used for the alkaline treatment of the present invention are preferably ammonia water and hydrogen peroxide; the concentration of the ammonia water is preferably 0.8-0.9 g / mL, specifically 0.8 g / mL, 0.85 g / mL or 0.9 g / mL; the concentration of the hydrogen peroxide is preferably 30-35 wt%, specifically 30 wt%, 32 wt% or 35 wt%; the volume ratio of the ammonia water to the hydrogen peroxide is preferably 1-3:1-2, more preferably 1:1. The alkaline treatment of the present invention is preferably carried out under ultrasonic conditions; the time of the alkaline treatment is preferably 10-15 min, more preferably 10-12 min. The present invention removes the acid solution remaining on the surface of the substrate by alkaline treatment. After the alkaline treatment, the present invention preferably dries the obtained substrate to obtain a pretreated substrate. In the present invention, the drying is preferably spin drying, and the spin drying speed is preferably 4000-4500 rpm, specifically 4000 rmp, 4200 rmp or 4500 rmp; the spin drying time is preferably 20-30 s, more preferably 25 s.
[0041] After obtaining the pre-treated substrate, the present invention applies photoresist on the upper surface of the pre-treated substrate to form a photoresist mask layer to obtain a photoresist substrate. In the present invention, the rotation rate of the carrier used during the coating is preferably 3000-3200rpm, specifically 3000rpm, 3100rpm or 3200rpm; the thickness of the photoresist mask layer is preferably 550-650nm, more preferably 600nm. After the photoresist coating is completed, the present invention preferably performs a hardening operation on the substrate coated with the photoresist to form a photoresist mask layer. In the present invention, the temperature of the hardening operation is preferably 80-85°C, more preferably 80-82°C; the time of the hardening operation is preferably 10-12min, specifically 10min, 11min or 12min.
[0042] After obtaining the photoresist substrate, the present invention sequentially exposes and develops the photoresist mask layer of the photoresist substrate to form a circular hole array in the photoresist mask layer, thereby obtaining a photoresist development substrate. In the present invention, the intensity of the light used for the exposure is preferably 2.0 to 2.1 mW / cm 2 , more preferably 2.0 W / cm 2 ; The exposure time is preferably 10 to 12 seconds, specifically 10 seconds, 11 seconds or 12 seconds. In the present invention, the development time is preferably 30 to 35 seconds, specifically 30 seconds, 31 seconds, 32 seconds, 33 seconds, 34 seconds or 35 seconds. The present invention transfers the graphic information on the photolithography plate to the photoresist mask layer by exposure; the photoresist mask layer forms a circular hole array by development. In the present invention, the circular hole array is formed by a plurality of circular holes that do not contact each other, the bottom surface of each circular hole exposes the substrate, and the photoresist mask layer is retained outside the circular hole. The diameter of the circular hole of the present invention is preferably 375 to 425 nm, more preferably 400 nm; the period (the distance between the centers of adjacent circular holes) is preferably 580 to 620 nm, more preferably 600 nm; the depth is preferably 600 to 605 nm, more preferably 600 nm.
[0043] After obtaining the photoresist development substrate, the present invention prepares an aluminum oxide film on the upper surface of the photoresist development substrate by atomic layer deposition to obtain an aluminum oxide film-coated substrate. In the present invention, the thickness of the aluminum oxide film is preferably 390 to 410 nm, more preferably 400 nm; the coating rate of the aluminum oxide film is preferably More preferably
[0044] After obtaining the aluminum oxide film-coated substrate, the present invention removes the remaining photoresist mask layer on the aluminum oxide film-coated substrate and the aluminum oxide film on the upper surface of the photoresist mask layer, retains the aluminum oxide film in each circular hole as an aluminum oxide cylinder, and obtains an aluminum oxide cylinder array formed by aluminum oxide cylinders on the upper surface of the substrate, with the substrate exposed between adjacent aluminum oxide cylinders. The present invention preferably removes the remaining photoresist mask layer on the aluminum oxide film-coated substrate and the aluminum oxide film on the upper surface of the remaining photoresist mask layer by microwave plasma degumming. In the present invention, the diameter of the aluminum oxide cylinder is the same as the diameter of the circular hole, and the height of the aluminum oxide cylinder is the same as the thickness of the aluminum oxide film.
[0045] After obtaining the aluminum oxide cylinder array formed by the aluminum oxide cylinders, the present invention prepares a gold film on the top and side walls of the aluminum oxide cylinders and the exposed upper surface of the substrate between adjacent aluminum oxide cylinders by electron beam evaporation to obtain a gold-plated substrate. In the present invention, the thickness of the gold film is preferably 38 to 42 nm, more preferably 40 nm; the evaporation rate of the gold film is preferably More preferably
[0046] After obtaining the gold-plated substrate, the present invention removes the gold film on the top of each aluminum oxide cylinder and the upper surface of the substrate between adjacent aluminum oxide cylinders on the gold-plated substrate by vertical etching, and retains the gold film on the side wall of the aluminum oxide cylinder. In the present invention, the conditions of the vertical etching preferably include: the angle of the stage is preferably 0°, the argon gas flow rate is preferably 8-10 sccm, more preferably 8 sccm; the time of the vertical etching is preferably 12-18 min, more preferably 15 min.
[0047] After the vertical etching, the present invention removes the aluminum oxide cylinder array by wet etching, and obtains a gold nanoring array formed by the remaining gold film on the upper surface of the substrate. In the present invention, the reagent used for the wet etching is preferably an aqueous phosphoric acid solution, and the mass fraction of the aqueous phosphoric acid solution is preferably 2-4%, more preferably 3%. The temperature of the wet etching of the present invention is preferably 70-75°C, more preferably 70-72°C. In the gold nanoring array of the present invention, the outer diameter of the gold nanoring is preferably 470-490nm, more preferably 480nm; the inner diameter is preferably 390-410nm, more preferably 400nm; the height is preferably 380-420nm, more preferably 400nm.
[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] The glass substrate of the embodiment is a 4-inch glass wafer.
[0050] Example 1
[0051] (1) The glass substrate was immersed in a mixed solution of concentrated sulfuric acid (98 wt%) and hydrogen peroxide (30 wt%) (the volume ratio of concentrated sulfuric acid to hydrogen peroxide was 2:1) and ultrasonically treated for 15 min to remove organic matter and metal particle impurities remaining on the surface of the glass substrate. Then, the glass substrate was immersed in a mixed solution of ammonia (0.8 g / mL) and hydrogen peroxide (30 wt%) (the volume ratio of ammonia to hydrogen peroxide was 1:1) and ultrasonically treated for 10 min to remove the acid remaining on the surface of the glass substrate. After the immersion treatment, the glass substrate was placed on a spin dryer and spun at a speed of 4500 rpm for 25 seconds to obtain a pretreated glass substrate.
[0052] (2) The pre-treated glass substrate is placed on a coating machine, and a layer of photoresist with a thickness of 600 nm is coated on the upper surface of the pre-treated glass substrate. After that, the glass substrate coated with the photoresist is placed in an oven and kept at 80° C. for 10 minutes to remove excess organic solvent in the photoresist and complete the vertical film operation, that is, a photoresist mask layer (with a thickness of 600 nm) is formed on the upper surface of the glass substrate to obtain a photoresist glass substrate, such as Figure 1 The photoresist glass substrate is placed in a photolithography machine and the light intensity is 2.0 mW / cm 2 The photoresist mask layer is exposed for 12 seconds under the conditions of , so as to transfer the graphic information on the photolithography plate to the photoresist mask layer; and then the development is performed, and the development time is 30 seconds, so that the photoresist mask layer forms a circular hole array, and a photoresist development glass substrate is obtained; the circular hole array is formed by a plurality of circular holes that do not contact each other, the bottom surface of each circular hole exposes the substrate, and the photoresist mask layer is retained outside the circular hole; the diameter of the circular hole is 400nm, the period is 600nm, and the depth is 600nm, such as Figure 1 as shown in (b).
[0053] (3) A layer of aluminum oxide film with a thickness of 400 nm is deposited on the upper surface of the photoresist developing glass substrate by atomic layer deposition. The deposition rate of the aluminum oxide film is Obtain an aluminum oxide film-coated substrate, such as Figure 2 After the deposition is completed, the remaining photoresist mask layer on the aluminum oxide film-coated substrate and the aluminum oxide film on the surface of the photoresist mask layer are removed by microwave plasma stripping, and the aluminum oxide film in each circular hole is retained as an aluminum oxide cylinder, and an aluminum oxide cylinder array formed by aluminum oxide cylinders is obtained on the upper surface of the glass substrate, and the glass substrate is exposed between adjacent aluminum oxide cylinders; the diameter of the aluminum oxide cylinder is 400nm, and the height is 400nm, as shown in FIG. Figure 2 as shown in (b).
[0054] (4) A gold film with a thickness of 40 nm was deposited on the top and side walls of the alumina cylinder and the exposed upper surface of the glass substrate between adjacent alumina cylinders by electron beam evaporation. The evaporation rate of the gold film was Get a gold-plated glass substrate, such as Figure 3 Then the gold-coated glass substrate is placed in a reactive ion beam etcher (RIBE) for vertical etching to remove the gold film on the top of each alumina cylinder on the gold-coated glass substrate and the upper surface of the glass substrate between adjacent alumina cylinders, and retain the gold film on the side wall of the alumina cylinder, as shown in FIG. Figure 3 As shown in (b); the specific operation of the vertical etching is as follows: the angle of the stage is set to 0°, and the gold-coated glass substrate is etched for 15 minutes under the condition of 8sccm argon gas flow. After the vertical etching is completed, the obtained glass substrate is placed in a 3% phosphoric acid aqueous solution and wet-etched at 75°C to remove the aluminum oxide cylinder array; after the wet etching is completed, a gold nanoring array formed by the remaining gold film (i.e., the gold film on the side wall of the aluminum oxide cylinder) is obtained on the upper surface of the glass substrate, as shown in FIG. Figure 4 shown.
[0055] In the gold nanoring array, the outer diameter of the gold nanoring is 480 nm, the inner diameter is 400 nm, and the height is 400 nm.
[0056] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a gold nanoring array, characterized in that: The following steps are involved: Applying photoresist on the upper surface of the substrate to form a photoresist mask layer; sequentially exposing and developing the photoresist mask layer to form a circular hole array in the photoresist mask layer, thereby obtaining a photoresist development substrate; The circular hole array is formed by a plurality of circular holes that are not in contact with each other, the bottom surface of each circular hole exposes the substrate, and a photoresist mask layer is retained outside the circular hole; An aluminum oxide film is prepared on the upper surface of the photoresist development substrate by atomic layer deposition, the remaining photoresist mask layer and the aluminum oxide film on the upper surface of the photoresist mask layer are removed, and the aluminum oxide film in each circular hole is retained as an aluminum oxide column, and an aluminum oxide column array formed by the aluminum oxide columns is obtained on the upper surface of the substrate, and the substrate is exposed between adjacent aluminum oxide columns; A gold film is prepared on the top and side wall of the alumina cylinder and the exposed upper surface of the substrate between adjacent alumina cylinders by electron beam evaporation to obtain a gold-plated substrate; The gold film on the top of each alumina cylinder and the upper surface of the substrate between adjacent alumina cylinders on the gold-plated substrate is removed by vertical etching, and the gold film on the side wall of the alumina cylinder is retained; The aluminum oxide column array is removed by wet etching to obtain a gold nano-ring array formed by the remaining gold film on the upper surface of the substrate.
2. The preparation method according to claim 1, characterized in that: The substrate includes a glass substrate, a silicon substrate, a gallium nitride substrate, a silicon carbide substrate or a gallium oxide substrate.
3. The preparation method according to claim 1, characterized in that: The thickness of the photoresist mask layer is 550-650 nm; the rotation rate of the carrier used during the coating is 3000-3200 rpm.
4. The preparation method according to claim 1, characterized in that: The intensity of the light used for the exposure is 2.0-2.1 mW / cm 2 The exposure time is 10 to 12 seconds, and the development time is 30 to 35 seconds.
5. The preparation method according to claim 1, characterized in that: The circular holes have a diameter of 375-425 nm, a period of 580-620 nm, and a depth of 600-605 nm.
6. The preparation method according to claim 1, characterized in that: The thickness of the aluminum oxide film is 390-410 nm, and the coating rate of the aluminum oxide film is 7. The preparation method according to claim 1, characterized in that: The thickness of the gold film is 38-42 nm, and the evaporation rate of the gold film is 8. The preparation method according to claim 1, characterized in that: The conditions for the vertical etching include: the angle of the stage is 0°, the flow rate of argon gas is 8-10 sccm; and the time for the vertical etching is 12-18 minutes.
9. The preparation method according to claim 1, characterized in that: The reagent used for the wet etching is a phosphoric acid aqueous solution, and the mass fraction of the phosphoric acid aqueous solution is 2-4%; the temperature of the wet etching is 70-75°C.
10. The preparation method according to claim 1 or 9, characterized in that: The method includes sequentially subjecting the substrate to an acid treatment and an alkali treatment before coating the photoresist on the substrate surface; The reagents used for the acid treatment are concentrated sulfuric acid and hydrogen peroxide, the concentration of the concentrated sulfuric acid is 98wt%, the concentration of the hydrogen peroxide is 30wt%-35wt%, and the volume ratio of the concentrated sulfuric acid to the hydrogen peroxide is 1-3:1-2; the time of the acid treatment is 10-20min; The reagents used for the alkali treatment are ammonia water and hydrogen peroxide. The concentration of the ammonia water is 0.8-0.9 g / mL, the concentration of the hydrogen peroxide is 30wt%-35wt%, and the volume ratio of the ammonia water to the hydrogen peroxide is 1-3:1-2. The time of the alkali treatment is 10-15 minutes.
Citation Information
Cited By
Preparation method of gold nano array coupled photonic crystal microcavity based on Tamm plasmon mode
CN119776945A