Preparation method of folic acid-based laser-induced graphene and flexible strain sensor
By using folic acid as the raw material for laser induction method, folate-based laser-induced graphene with excellent performance was prepared, which solved the high cost and pollution problems of traditional graphene preparation methods, and achieved high sensitivity and wide application of flexible graphene strain sensors.
Patent Information
- Application Number
- CN202411118994.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing graphene preparation methods have high costs, pollution problems and unstable performance. The laser induction method uses polyimide films and is environmentally contaminated, and lacks flexible graphene strain sensor devices with excellent performance.
Folic acid is used as the raw material for the laser induction method, and folic acid solution is prepared by preparing polyvinyl alcohol solution and folic acid solution to form a film and laser induction graphene, and a flexible strain sensor with an H-shaped structure is formed by combining a flexible substrate and a conductive silver liquid.
It reduces the production cost of graphene, improves the conductivity and sensitivity, realizes real-time detection of strain changes of 0-13%, has efficient conductive electrical signals and sewage adsorption and filtration functions, and the sensor structure is simple and environmentally friendly.
Smart Images

Figure CN119018883A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene materials, and in particular relates to a preparation method of folic acid-based laser-induced graphene and a flexible strain sensor. Background Art
[0002] Graphene is a single-atom-thick flat sheet and a special two-dimensional structural material. 2 Carbon atoms connected by bonds form a honeycomb lattice. Since graphene was first produced by Andre Geim and Konstantin Novoselov using mechanical exfoliation in 2004, its superior properties have attracted strong attention from scientists around the world. Graphene has a specific surface area of 2500-3000m 2 / g; the mechanical and electrical properties of graphene are also very good at room temperature; the mechanical strength is up to 10 12 Pa, which is almost 5 times that of steel; the resistivity of graphene is only 1×10 -6 Ω·cm; its light transmittance is as high as 98%. These superior performance characteristics make graphene widely used in energy storage devices (supercapacitors, batteries), sensors (chemical sensors, physical sensors), environmental protection (wastewater adsorption), optical devices (biomedical imaging) and other fields. However, the promotion of graphene is limited by its preparation method. At present, the mainstream international graphene preparation methods include mechanical exfoliation, redox method, chemical vapor deposition method, laser induction method, etc. Mechanical exfoliation is the most traditional, with a very low yield and uneven quality of graphene produced; the redox method requires the use of a large amount of chemical reagents, which has pollution problems and explosion risks during the production process; the chemical vapor deposition method has very high requirements for equipment and the reaction is usually carried out at nearly 1,000 degrees Celsius. In contrast, the laser induction method for preparing graphene is easy to operate, simple in process, and safer.
[0003] The laser induction method uses laser to irradiate the surface of a certain material film, and through the transient photothermal / photochemical composite effect, the hybrid amorphous carbon sp 3 -C is converted into conductive sp 2-C is a method for making graphene. Its preparation process is simple and fast, avoiding the problems of expensive reaction systems and complex processing processes in traditional graphene production methods, and has extremely high development prospects. However, most of the raw materials used for preparing graphene by laser induction are polyimide films. Polyimide film is made by polycondensing and casting pyromellitic anhydride (PMDA) and diaminodiphenyl ether (ODA) in a very strong solvent dimethylacetamide (DMAC), and then imidizing. The preparation process is relatively complicated, the cost is relatively high, and there are pollution problems. At present, some studies use degradable materials such as lignin and sugar polyshell hydrochloride as raw materials for laser-induced preparation of graphene, but either the raw materials are expensive or the output graphene has poor performance and is unstable. Therefore, it is urgent to find a new material that can replace polyimide film. The characteristics of this material should be: easy to prepare and low preparation cost, the preparation process is completely green or has only a small amount of pollution emissions, and the molecular structure contains aromatic hydrocarbons that are easy to absorb laser energy.
[0004] Folic acid (molecular formula is C 19 H 19 N7O6), commonly known as vitamin B, also known as vitamin M, vitamin Be, also known as pteroylglutamate. It is commonly found in some fruits (citrus), yeast and green vegetables in nature. At present, the main methods of folic acid extraction are single enzyme method, three enzyme method, ultrasonic extraction method and water bath extraction method. The single enzyme method is mainly suitable for samples with less sugar and protein, such as spinach, beans and cabbage. The three enzyme method is mainly suitable for extracting samples rich in carbohydrates and proteins. Folic acid can be extracted from industrial and agricultural waste. The research team of Angel Bio Group in Yichang, Hubei extracted folic acid from waste beer yeast. The team of Li Fulan of Sichuan University of Technology extracted folic acid from silkworm feces. Folic acid is a light yellow crystal, and its color is determined by the presence of para-aminobenzoic acid structural units in the molecule. This structural unit is an aromatic compound containing a benzene ring. Aromatic compounds usually have relatively strong absorption and emission spectra, with a maximum absorption wavelength of 265nm. Therefore, compared with other raw materials, folic acid can better absorb the energy of the laser when it is induced by laser for surface modification, thereby greatly improving production efficiency and reducing energy loss in the production process. In addition, the molecular structure of folic acid contains aromatics, which are easier to transform into graphene structures under the high temperature and high pressure conditions brought by the laser.
[0005] In the prior art, there has been no report on a technical solution for using folic acid as the main raw material for preparing graphene by laser induction method.
[0006] In the current research on strain sensors, sensors using metal and semiconductor materials as sensitive elements have high accuracy, but lack ductility, cannot measure strains in a large range, and have a narrow application range; sensors using new generation materials such as metal nanoparticles and carbon nanotubes as sensitive elements have complex structures and are difficult to prepare. The existing technology lacks flexible graphene strain sensor devices with excellent performance and simple structure. Summary of the invention
[0007] In view of the above technical problems, one object of the present invention is to provide a method for preparing folic acid-based laser-induced graphene, using folic acid as the main raw material for preparing graphene by laser induction, thereby reducing production costs, enhancing conductivity and reducing environmental pollution.
[0008] Another object of the present invention is to provide folate-based laser-induced graphene prepared by the above method.
[0009] Another object of the present invention is to provide a folate-based laser-induced graphene flexible strain sensor, which uses the folate-based laser-induced graphene of the present invention as a sensitive element, has electrodes connected on both sides, has a simple structural design, and can respond to strain changes of the object being measured in real time.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] A method for preparing folic acid-based laser-induced graphene comprises the following steps:
[0012] S1. Prepare polyvinyl alcohol solution:
[0013] Polyvinyl alcohol and deionized water are mixed at a mass ratio of 1:10 using a constant temperature magnetic stirrer to form a polyvinyl alcohol solution;
[0014] S2. Prepare a mixed solution of folic acid, alkali solution and polyvinyl alcohol solution:
[0015] Mix folic acid, an alkaline solution with a concentration of 1% to 5%, and the polyvinyl alcohol solution prepared in step S1 in the following ratios: the mass ratio of the folic acid to the alkaline solution is 1:2 to 40, and the mass ratio of the alkaline solution to the polyvinyl alcohol solution is 1:1;
[0016] S3, defoaming the blended liquid to obtain a folic acid solution;
[0017] S4, forming a film of the folic acid solution to obtain a folic acid-based film:
[0018] The film is formed by a solution casting method, the folic acid solution obtained in step S3 is transferred to a film-forming mold, and then dried to obtain a folic acid-based film;
[0019] S5. Preparing folic acid-based laser-induced graphene from the folic acid-based film by laser induction:
[0020] The laser induction is direct laser irradiation; the direct laser irradiation is performed in an intelligent laser engraving machine; the laser intensity of the intelligent laser engraving machine is 3-5W, the laser wavelength is 460nm; and the irradiation rate is 110mm / s.
[0021] In the step S1, the polyvinyl alcohol is white crystalline particles of polyvinyl alcohol with a molar mass of 146000 to 186000, the speed of the constant temperature magnetic stirrer is 150 to 200 rpm, the stirring temperature is 80 to 90° C., and the stirring time is 25 to 40 min.
[0022] In the step S2, the mass ratio of the folic acid to the alkaline solution is 1:20, 1:10, 3:20, 1:5 or 1:4; the folic acid is a yellow solid powder of folic acid; the alkaline solution is a sodium hydroxide solution with a concentration of 2%; the folic acid, the alkaline solution and the polyvinyl alcohol solution are mixed uniformly using a constant temperature magnetic stirrer; the speed of the constant temperature magnetic stirrer is 150-200 rpm; the stirring temperature is 25-30°C; and the stirring time is 15-20 min.
[0023] In the step S3, the defoaming is vacuum defoaming; the vacuum defoaming is carried out in an acrylic vacuum box; and the defoaming time is 15 to 20 minutes.
[0024] In the step S4, the amount of folic acid solution transferred is: 10 mL of folic acid solution is transferred to a film-forming mold with a diameter of 9 cm; the drying is carried out in a constant temperature forced air drying oven; the drying temperature is 20 to 30° C.; and the drying time is 8 to 24 hours.
[0025] In step S5, the laser intensity of the intelligent laser engraving machine is 3.25W, 3.5W, 3.75W, 4W or 4.25W; the distance between the laser source of the intelligent laser engraving machine and the folic acid-based film is 4 cm.
[0026] The sheet resistance of the folic acid-based laser-induced graphene is 91.2-271.9Ω / Sq, the crystallite size is 6.42-15.98nm, and the intensity ratio of the Raman spectrum is 1 D / I G 1.18~2.96, I 2D / I G It is 0.07~1.50.
[0027] A folate-based laser-induced graphene prepared by utilizing the method for preparing folate-based laser-induced graphene.
[0028] A flexible strain sensor prepared by using folic acid-based laser induced graphene comprises a flexible substrate 1, a strain sensing region 2, a conductive silver liquid coating region 3 and an electrode region 4; the folic acid-based laser induced graphene is transferred and fixed on the upper surface of the flexible substrate 1 to form the strain sensing region 2; the conductive silver liquid is applied to both ends of the strain sensing region 2 to form two conductive silver liquid coating regions 3; a conductive copper foil is attached to each conductive silver liquid coating region 3 to form two electrode regions 4, and the two electrode regions 4 are connected to each other through the strain sensing region 2 to form an "H"-shaped structure.
[0029] Under a tensile strain change of 0-7%, the sensitivity of the flexible strain sensor is 24; under a tensile strain change of 7-11%, the sensitivity of the flexible strain sensor is 84; under a tensile strain change of 11-13%, the sensitivity of the flexible strain sensor is 361.
[0030] Compared with the prior art, the beneficial effects of the present invention are: the folic acid-based laser-induced graphene of the present invention has good electrical conductivity and a loose porous structure, has the characteristics of efficient conduction of electrical signals and strong adsorption, and can realize the functions of electrodes, supercapacitors, and sewage adsorption and filtration.
[0031] The folic acid-based laser-induced graphene prepared by the method of the present invention has the following advantages:
[0032] 1) Significantly improve the performance of traditional laser-induced graphene and increase its utilization rate;
[0033] 2) Reducing the production cost of laser-induced graphene and improving economic benefits are of great significance for the promotion of graphene materials in my country;
[0034] 3) Reduce the use of chemical reagents and try to avoid adverse effects on the environment during the production process;
[0035] 4) Utilize folic acid in agricultural products as a resource, increase the utilization rate of folic acid and improve added value.
[0036] Using folic acid as the main raw material for preparing graphene by laser induction can improve production efficiency, reduce production costs, and improve conductivity. Compared with the traditional production process using polyimide as raw material and the new production process using lignin and sugar polyshell hydrochloride as raw materials, it can greatly reduce pollution and damage to the environment and reduce costs.
[0037] The flexible strain sensor based on folic acid-based laser-induced graphene of the present invention has the following advantages:
[0038] 1) Compared with the existing flexible graphene strain sensor, the flexible strain sensor based on folic acid-based laser-induced graphene of the present invention has lower preparation cost, simpler steps and less pollution to the environment.
[0039] 2) The flexible strain sensor of the present invention has a wide strain detection range, reaching a strain variation range of 0-13%, and can respond in real time to everything from tiny deformations to large movements, and has a broad application prospect.
[0040] 3) The flexible strain sensor substrate of the present invention uses a flexible material, which can better adhere to the outer surface of the object being measured and has higher accuracy and wearability.
[0041] 4) After 10,000 repeated stretchings, the flexible strain sensor of the present invention has a stable strain variation range, and the stretching curve and the recovery curve can still undergo stable periodic changes according to the stretching amplitude, indicating that it has stable performance and a long service life.
[0042] 5) The resistance strain variation range of the flexible strain sensor of the present invention is the same under different pulling speeds, indicating that the strain sensor can work normally under different stretching conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a step diagram of the method for preparing folate-based laser-induced graphene of the present invention.
[0044] Figure 2 This is a Raman spectrum image of the folic acid-based laser-induced graphene prepared in Examples 1-5 of the present invention.
[0045] Figure 3 This is the Raman spectrum image of the folic acid-based laser-induced graphene prepared in Examples 3 and 6-9 of the present invention.
[0046] Figure 4 This is a scanning electron microscope image of the folic acid-based film prepared in Example 8 of the present invention.
[0047] Figure 5 This is a scanning electron microscope image of the folic acid-based laser-induced graphene prepared in Example 8 of the present invention;
[0048] Figure 6 This is a schematic diagram of the structure of a folic acid-based graphene flexible strain sensor prepared in Example 10 of the present invention;
[0049] Figure 7 This is a resistance strain change diagram of the folic acid-based graphene flexible strain sensor prepared in Example 10 of the present invention after repeated stretching 10,000 times;
[0050] Figure 8 This is a sensitivity change diagram of the folic acid-based graphene flexible strain sensor prepared in Example 10 of the present invention under different strains;
[0051] Fig. 9This is a graph showing the resistance strain variation at different stretching rates of the folic acid-based graphene flexible strain sensor prepared in Example 10 of the present invention.
[0052] The accompanying drawings are denoted as follows:
[0053] 1 Flexible substrate
[0054] 2 Strain Sensing Area
[0055] 3Conductive silver liquid coating area
[0056] 4 electrode areas DETAILED DESCRIPTION
[0057] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0058] The method for preparing folate-based laser-induced graphene provided by the present invention comprises the following steps:
[0059] S1. prepare polyvinyl alcohol solution;
[0060] Polyvinyl alcohol and deionized water are mixed in a mass ratio of 1:10 using a constant temperature magnetic stirrer to form a polyvinyl alcohol solution; the polyvinyl alcohol is white crystalline particles of polyvinyl alcohol with a molar mass of 146000 to 186000; wherein the speed of the constant temperature magnetic stirrer is 150 to 200 rpm, the stirring temperature is 80 to 90° C., preferably 85° C.; and the stirring time is 25 to 40 min, preferably 30 min.
[0061] S2, preparing a mixed solution of folic acid, alkaline solution and polyvinyl alcohol solution;
[0062] Folic acid, an alkaline solution with a concentration of 1% to 5%, and the polyvinyl alcohol solution prepared in step S1 are uniformly mixed in proportion, wherein the mass ratio of the folic acid to the alkaline solution is 1:2 to 40, preferably 1:20, 1:10, 3:20, 1:5 or 1:4; the mass ratio of the alkaline solution to the polyvinyl alcohol solution is 1:1;
[0063] The folic acid is yellow solid folic acid powder.
[0064] Preferably, the alkaline solution is a sodium hydroxide solution with a concentration of 2%.
[0065] Preferably, the folic acid, the alkaline solution and the polyvinyl alcohol solution are uniformly mixed using a constant temperature magnetic stirrer; the rotation speed of the constant temperature magnetic stirrer is 150-200 rpm; the stirring temperature is 25-30° C.; and the stirring time is 15-20 min.
[0066] S3, defoaming the blended liquid to obtain a folic acid solution;
[0067] The defoaming is vacuum defoaming;
[0068] The vacuum defoaming is carried out in an acrylic vacuum box; the defoaming time is 15 to 20 minutes.
[0069] S4, forming a film of the folic acid solution to obtain a folic acid-based film;
[0070] The film is formed by solution casting, and the specific steps are as follows:
[0071] The folic acid solution obtained in step S3 is transferred to a film-forming mold, and then dried to obtain a folic acid-based film;
[0072] The amount of the folic acid solution transferred is: 10 mL of the folic acid solution is transferred to a film-forming mold having a diameter of 9 cm;
[0073] Preferably, the drying is carried out in a constant temperature forced air drying oven; the drying temperature is 20 to 30° C., preferably 25° C.; the drying time is 8 to 24 hours, preferably 12 hours.
[0074] S5, preparing the folic acid-based film into folic acid-based laser-induced graphene by laser induction;
[0075] The laser induction is direct laser irradiation;
[0076] The laser direct irradiation is carried out in an intelligent laser engraving machine;
[0077] The laser intensity of the intelligent laser engraving machine is 3-5W, specifically 3.25W, 3.5W, 3.75W, 4W, 4.25W;
[0078] The laser wavelength of the intelligent laser engraving machine is 460nm;
[0079] The irradiation rate of the intelligent laser engraving machine is 110 mm / s;
[0080] The distance between the laser source of the intelligent laser engraving machine and the folic acid-based film is 4 cm.
[0081] The folic acid-based laser-induced graphene has good electrical conductivity, microstructure, high mechanical strength, high specific surface area and adsorption performance; the sheet resistance of the folic acid-based laser-induced graphene is 91.2-271.9Ω / Sq, and the crystallite size is 6.42-15.98nm. Compared with the original technology using polyimide film as raw material, the sheet resistance of the present invention is reduced by about 62.8%.
[0082] The folic acid-based laser-induced graphene of the present invention has a wide range of raw material sources, low prices and low production costs. The folic acid-based laser-induced graphene can utilize folic acid as a resource and improve its added value. The folic acid-based laser-induced graphene reduces the use of chemical reagents and can effectively reduce the adverse consequences caused by chemical reagent residues in the process of preparing graphene.
[0083] A folic acid-based laser-induced graphene flexible strain sensor comprises a flexible substrate 1, a strain sensing region 2, a conductive silver liquid coating region 3 and an electrode region 4; the folic acid-based laser-induced graphene is transferred and fixed on the upper surface of the flexible substrate 1 to form the strain sensing region 2; the conductive silver liquid is applied to both ends of the strain sensing region 2 to form two conductive silver liquid coating regions 3; a conductive copper foil is attached to each conductive silver liquid coating region 3 to form two electrode regions 4, and the two electrode regions 4 are connected to each other through the strain sensing region 2 to form an "H"-shaped structure.
[0084] The concentration of the conductive silver liquid is 10%-50%.
[0085] The length of the flexible substrate 1 is 40.0±5 mm, and the width is 20±2 mm; the length of the strain sensing area 2 is 25.0±0.5 mm, and the width is 10.0±0.5 mm.
[0086] Preferably, the flexible substrate 1 is an Ecoflex (ecological flexible substrate) substrate or a PDMS (polydimethylsiloxane) substrate.
[0087] Preferably, the electrode region 4 may be rectangular, square or irregular in shape.
[0088] The strain sensing region 2 is formed by the following method:
[0089] Use a spin coater to evenly coat PDMS (polydimethylsiloxane) glue on the folic acid-based laser induced graphene of the present invention, with a rotation speed of 2000 rpm and an angular acceleration speed of 500 rpm / s. After evenly spin coating, put it in a 35°C oven for drying for 30 minutes, and then put it in deionized water for 15 minutes to separate the folic acid-based laser induced graphene from the folic acid-based film and transfer it to the flexible substrate 1. Put the folic acid-based laser induced graphene / flexible substrate composite material in a 35°C convection oven for drying for 20 minutes, and then cut the flexible substrate 1 into 40×20 mm.
[0090] Preferably, conductive silver liquid is applied to 5 mm×20 mm at both ends of the strain sensing region 2 to form a conductive silver liquid coating region 3 .
[0091] Preferably, after pasting the conductive copper foil on the conductive silver liquid coating area 3, it is placed in the air for air drying for 1 hour to prepare a folic acid-based graphene flexible strain sensor.
[0092] The folic acid-based graphene flexible strain sensor has high sensitivity and is made of flexible materials, which can fit tightly to the surface of the object being measured. It has strong wearability and can be used for human health monitoring (swallowing, breathing, joint movements, etc.) and virtual reality technology.
[0093] Example 1
[0094] 1. Prepare polyvinyl alcohol solution
[0095] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0096] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0097] Accurately weigh 0.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0098] 3. Defoam the blended liquid to obtain a folic acid solution
[0099] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0100] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0101] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0102] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0103] The folic acid-based film was peeled off from the mold and placed flat in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.5 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0104] Example 2
[0105] 1. Prepare polyvinyl alcohol solution
[0106] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0107] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0108] Accurately weigh 1.00 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0109] 3. Defoam the blended liquid to obtain a folic acid solution
[0110] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0111] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0112] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0113] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0114] The folic acid-based film was peeled off from the mold and placed flat in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.5 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0115] Example 3
[0116] 1. Prepare polyvinyl alcohol solution
[0117] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0118] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0119] Accurately weigh 1.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0120] 3. Defoam the blended liquid to obtain a folic acid solution
[0121] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0122] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0123] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0124] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0125] The folic acid-based film was peeled off from the mold and placed flat in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.5 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0126] Example 4
[0127] 1. Prepare polyvinyl alcohol solution
[0128] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0129] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0130] Accurately weigh 2.00 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0131] 3. Defoam the blended liquid to obtain a folic acid solution
[0132] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0133] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0134] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0135] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0136] The folic acid-based film was peeled off from the mold and placed flat in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.5 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0137] Example 5
[0138] 1. Prepare polyvinyl alcohol solution
[0139] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0140] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0141] Accurately weigh 2.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0142] 3. Defoam the blended liquid to obtain a folic acid solution
[0143] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0144] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0145] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0146] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0147] The folic acid-based film was peeled off from the mold and placed flat in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.5 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0148] Example 6
[0149] 1. Prepare polyvinyl alcohol solution
[0150] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0151] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0152] Accurately weigh 1.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0153] 3. Defoam the blended liquid to obtain a folic acid solution
[0154] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0155] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0156] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0157] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0158] The folic acid-based film was peeled off from the mold and placed flatly in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.25 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0159] Example 7
[0160] 1. Prepare polyvinyl alcohol solution
[0161] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0162] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0163] Accurately weigh 1.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0164] 3. Defoam the blended liquid to obtain a folic acid solution
[0165] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0166] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0167] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0168] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0169] The folic acid-based film was peeled off from the mold and placed flatly in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 3.75 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0170] Example 8
[0171] 1. Prepare polyvinyl alcohol solution
[0172] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0173] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0174] Accurately weigh 1.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0175] 3. Defoam the blended liquid to obtain a folic acid solution
[0176] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0177] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0178] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0179] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0180] The folic acid-based film was peeled off from the mold and placed flatly in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 4 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0181] Example 9
[0182] 1. Prepare polyvinyl alcohol solution
[0183] Take 20 g of polyvinyl alcohol and pour it into a beaker containing 200 mL of deionized water. Use a constant temperature magnetic stirrer to maintain the temperature at 85°C and stir at 200 rpm for 30 min.
[0184] 2. Prepare a blend of folic acid, alkaline solution and polyvinyl alcohol solution
[0185] Accurately weigh 1.50 g (accurate to 0.01 g) of folic acid, 10.0 g (accurate to 0.1 g) of 2% sodium hydroxide solution and 10.0 g (accurate to 0.1 g) of the above polyvinyl alcohol solution into a beaker, use a constant temperature magnetic stirrer to maintain the temperature at 30°C, and stir at 200 rpm for 15 min to obtain a mixed solution.
[0186] 3. Defoam the blended liquid to obtain a folic acid solution
[0187] The beaker containing the mixed solution was placed in an acrylic vacuum box for defoaming, and the vacuum pump was turned on to evacuate the air pressure in the acrylic vacuum box to 0 and maintained for 15 minutes to obtain a folic acid solution.
[0188] 4. Form the folic acid solution into a film to obtain a folic acid-based film
[0189] 10 mL of folic acid solution was transferred with a pipette and evenly added into a film-forming mold with a diameter of 9 cm, and the mold was placed in an electric constant temperature forced air drying oven and dried at 25° C. for 12 h to obtain a folic acid-based film.
[0190] 5. Preparation of folic acid-based film into folic acid-based laser-induced graphene by laser induction
[0191] The folic acid-based film was peeled off from the mold and placed flatly in the intelligent laser engraving machine, with the distance between the laser emission source of the engraving machine and the folic acid-based film being 4 cm. The irradiation rate of the intelligent laser engraving machine was 110 mm / s, the laser power was 4.25 W, the laser wavelength was 460 nm, the laser irradiation area was 1 cm×1 cm, and the laser irradiation was carried out at an indoor temperature of 25°C and an indoor humidity of 40%, and light should be avoided.
[0192] Comparative Example
[0193] This comparative example refers to Examples 1-9, except that: when preparing the folic acid solution, the mass ratio of folic acid to alkaline solution is 1:50, the laser power during laser irradiation is 6 W, and the other components and their contents and preparation methods remain unchanged. The prepared sample is folic acid-based laser-induced graphene.
[0194] Performance testing of folic acid-based laser-induced graphene
[0195] 1. Electrical properties
[0196] (1) Square resistance test
[0197] HPS2523 coating square resistance tester (Beijing Jiahang Bochuang Technology Co., Ltd.) was used to test the square resistance of Examples 1-9 to determine the conductive properties of folic acid-based laser-induced graphene. The graphene was cut into a rectangle of 10×10 mm and laid flat on the table. The four corner probes of the square resistance tester were gently contacted with the graphene surface until the tester displayed the graphene square resistance. The test was repeated three times, and the results were averaged and expressed as mean ± standard deviation.
[0198] (2) Raman test
[0199] The Raman spectra of Examples 1-9 were tested using an inVia microscopic laser Raman spectrometer (Renishaw, UK) to determine the conductivity of the folate-based laser-induced graphene. The graphene was cut into a rectangle of 10×10 mm, placed in a Raman spectrometer and a laser emitting 532 nm laser was used at 500-3500 cm -1 The wave number range was scanned. The test was repeated three times and the results were averaged and expressed as mean ± standard deviation.
[0200] 2. Microstructure
[0201] The surface microstructure of Example 3 was observed using a JSM-56700F scanning electron microscope (JEOL Ltd.). The graphene was sprayed with gold and scanned in a high vacuum environment. The magnification of the folate film was 1000×, and the magnification of the folate laser-induced graphene was 2000×. The microscopic morphologies are shown in Figure 3. Figure 4 and Figure 5 shown.
[0202] The square resistance values of the folic acid-based laser-induced graphene described in Examples 1-9 are shown in the following table:
[0203] Table 1
[0204]
[0205] In Table 1, the crystallite size, I D / I G and I 2D / I G All by Figure 2 and Figure 3 The Raman spectrum test results show that the larger the crystallite size, the stronger the conductivity; D / I G The smaller, I 2D / I GThe larger the value, the smaller the surface defects of graphene and the better the conductivity. It can be seen from Examples 1-5 in Table 1 that with the increase of the amount of folic acid added, the conductivity of folic acid-based laser-induced graphene first increases and then decreases. It can be seen from Examples 3 and 6-9 in Table 1 that with the increase of laser intensity, the conductivity of folic acid-based laser-induced graphene first increases and then decreases. Example 8, i.e., the folic acid-based laser-induced graphene prepared by the process of 1.5g folic acid addition and 4W laser intensity has the best performance, and its square resistance is reduced by about 62.8% compared with the square resistance of the original technology using polyimide film as raw material.
[0206] from Figure 4 It can be seen that the microscopic surface of the folic acid-based film is uniform and flat, indicating that the preparation process of the folic acid-based film is mature and can meet the preparation requirements of folic acid-based laser-induced graphene.
[0207] from Figure 5 It can be seen that the folate-based laser-induced graphene has a foam-like porous structure. This is due to the rapid release of gas molecules (CO2, H2O) generated during the laser scribing of the raw materials, which leads to the formation of this hierarchical porous structure. This honeycomb porous structure is beneficial to improving its electrochemical performance. This is because it increases the accessible surface area, allowing the electrolyte to diffuse quickly into the electrode. This greatly enhances the conductive properties of the folate-based laser-induced graphene.
[0208] Example 10
[0209] Figure 6 The present invention is a structural schematic diagram of a folate-based graphene flexible strain sensor, wherein 1 is a PDMS flexible substrate, 2 is a strain sensing region, 3 is a conductive silver liquid coating region, and 4 is an electrode region, which can be connected to an external measuring device. Its working principle is that when the folate-based laser-induced graphene in the strain sensing region 2 is in a flat state, the length is L0, and its resistance value is the smallest, which is R0; when the strain sensor is deformed with the measured object, the length of the graphene in the strain sensing region 2 is L, the pores increase, and the resistance value increases to R. The resistance strain value (R-R0 / R0) of the strain sensor is determined by experiment to be linearly related to the tensile strain change (L-L0 / L0), so the resistance strain value of the strain sensor can reflect the tensile strain change in real time.
[0210] Figure 7 This is a resistance strain change graph of the folate-based graphene flexible strain sensor of the present invention after repeated stretching 10,000 times. After 10,000 times of repeated stretching, the resistance strain change of the folate-based graphene flexible strain sensor of the present invention still fluctuates periodically, and the stretching curve coincides with the recovery curve, and the strain detection function can still be performed, indicating that the folate-based graphene flexible strain sensor of the present invention has a long service life, high durability, high stability and excellent performance.
[0211] Figure 8 The present invention is a graph showing a change in sensitivity of the folate-based graphene flexible strain sensor of the present invention under a tensile strain change of 0-13%. The sensitivity of the folate-based graphene flexible strain sensor of the present invention under a tensile strain change of 0-7% is 24, the sensitivity of the folate-based graphene flexible strain sensor of the present invention under a tensile strain change of 7-11% is 84, and the sensitivity of the folate-based graphene flexible strain sensor of the present invention under a tensile strain change of 11-13% is 361, indicating that the folate-based graphene flexible strain sensor of the present invention can sense the area of 0-13% tensile strain change in real time, has a large detection range and high sensitivity.
[0212] Fig. 9 The present invention is a resistance strain change diagram of the folate-based graphene flexible strain sensor at stretching rates of 1 mm / s, 2 mm / s, and 3 mm / s. The experimental results show that the resistance strain values of the folate-based graphene flexible strain sensor of the present invention are maintained within the same range at different stretching rates, and the reaction strain change of the folate-based graphene flexible strain sensor of the present invention is not affected by the stretching rate, indicating that the folate-based graphene flexible strain sensor of the present invention has excellent performance and can cope with the detection of strain changes under different conditions.
Claims
1. A method for preparing folic acid-based laser-induced graphene, It is characterized in that The preparation method comprises the following steps: S1. Prepare polyvinyl alcohol solution: Polyvinyl alcohol and deionized water are mixed at a mass ratio of 1:10 using a constant temperature magnetic stirrer to form a polyvinyl alcohol solution; S2. Prepare a mixed solution of folic acid, alkali solution and polyvinyl alcohol solution: Mix folic acid, an alkaline solution with a concentration of 1% to 5%, and the polyvinyl alcohol solution prepared in step S1 in the following ratios: the mass ratio of the folic acid to the alkaline solution is 1:2 to 40, and the mass ratio of the alkaline solution to the polyvinyl alcohol solution is 1:1; S3, defoaming the blended liquid to obtain a folic acid solution; S4, forming a film of the folic acid solution to obtain a folic acid-based film: The film is formed by a solution casting method, the folic acid solution obtained in step S3 is transferred to a film-forming mold, and then dried to obtain a folic acid-based film; S5. Preparing folic acid-based laser-induced graphene from the folic acid-based film by laser induction: The laser induction is direct laser irradiation; the direct laser irradiation is performed in an intelligent laser engraving machine; the laser intensity of the intelligent laser engraving machine is 3-5W, the laser wavelength is 460nm; and the irradiation rate is 110mm / s.
2. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that In the step S1, the polyvinyl alcohol is white crystalline particles of polyvinyl alcohol with a molar mass of 146000 to 186000, the speed of the constant temperature magnetic stirrer is 150 to 200 rpm, the stirring temperature is 80 to 90° C., and the stirring time is 25 to 40 min.
3. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that In the step S2, the mass ratio of the folic acid to the alkaline solution is 1:20, 1:10, 3:20, 1:5 or 1:4; the folic acid is a yellow solid powder; the alkaline solution is a sodium hydroxide solution with a concentration of 2%; the folic acid, the alkaline solution and the polyvinyl alcohol solution are mixed uniformly using a constant temperature magnetic stirrer; the speed of the constant temperature magnetic stirrer is 150-200 rpm; the stirring temperature is 25-30°C; and the stirring time is 15-20 min.
4. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that In the step S3, the defoaming is vacuum defoaming; the vacuum defoaming is carried out in an acrylic vacuum box; and the defoaming time is 15 to 20 minutes.
5. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that In the step S4, the amount of folic acid solution transferred is: 10 mL of folic acid solution is transferred to a film-forming mold with a diameter of 9 cm; the drying is carried out in a constant temperature forced air drying oven; the drying temperature is 20 to 30° C.; and the drying time is 8 to 24 hours.
6. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that In step S5, the laser intensity of the intelligent laser engraving machine is 3.25W, 3.5W, 3.75W, 4W or 4.25W; the distance between the laser source of the intelligent laser engraving machine and the folic acid-based film is 4 cm.
7. The method for preparing folate-based laser-induced graphene according to claim 1, It is characterized in that The sheet resistance of the folic acid-based laser-induced graphene is 91.2-271.9Ω / Sq, the crystallite size is 6.42-15.98nm, and the intensity ratio of the Raman spectrum is 1 D / I G 1.18~2.96, I 2D / I G It is 0.07~1.
50.
8. Folate-based laser-induced graphene prepared by the method for preparing folate-based laser-induced graphene according to any one of claims 1 to 7.
9. A flexible strain sensor prepared using the folic acid-based laser-induced graphene according to claim 8, It is characterized in that The flexible strain sensor comprises a flexible substrate (1), a strain sensing region (2), a conductive silver liquid coating region (3) and an electrode region (4); folic acid-based laser-induced graphene is transferred and fixed on the upper surface of the flexible substrate (1) to form the strain sensing region (2); conductive silver liquid is applied to both ends of the strain sensing region (2) to form two conductive silver liquid coating regions (3); a conductive copper foil is attached to each conductive silver liquid coating region (3) to form two electrode regions (4); the two electrode regions (4) are connected to each other through the strain sensing region (2) to form an "H"-shaped structure.
10. The flexible strain sensor according to claim 9, It is characterized in that Under a tensile strain change of 0-7%, the sensitivity of the flexible strain sensor is 24; under a tensile strain change of 7-11%, the sensitivity of the flexible strain sensor is 84; under a tensile strain change of 11-13%, the sensitivity of the flexible strain sensor is 361.
Citation Information
Patent Citations
Planar supercapacitor and preparation method thereof
CN112735837A
Preparation method and application of graphene microelectrode based on smartphone detection
CN115452908A
Graphene heating film and preparation method thereof
CN115623617A
Fabric-based laser-induced graphene electric heating flexible film as well as preparation method and application thereof
CN117769068A
Thermoelectric Permingeatite Materials Double-Doped with Tin and Sulfur
KR102794386B1