Modified biochar composite material as well as preparation method and application thereof

Through the preparation of modified biochar composite materials, the use of nitrogen-doped biochar matrix to support cobalt nanoparticles to form Co-N bonds, solving the problems of high prices and low reserves of precious metal catalysts, and achieving efficient oxygen reduction and oxygen precipitation reaction catalysis , has promoted the commercial application of metal-air batteries.

CN119018890APending Publication Date: 2024-11-26BAOJI UNIV OF ARTS & SCI

Patent Information

Application Number
CN202411113795.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing precious metal catalysts have excellent performance but high prices and low reserves in oxygen reduction reactions (ORR) and oxygen precipitation reactions (OER), which hinders the commercial application of metal-air batteries.

Method used

Using modified biochar composite materials as catalysts, biochar is obtained by mixing and calcining the biomass raw material with a pore-forming agent, and then calcining it with a nitrogen source and a cobalt source to form a nitrogen-doped biochar matrix, and the cobalt nanoparticles are supported to form Co- N bonds improve conductivity and reactivity.

Benefits of technology

It achieves low-cost and efficient catalytic performance, which is better than commercially available Pt/C and Ir/C catalysts, and exhibits excellent kinetic performance in ORR and OER, reducing the production cost of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018890A_ABST
    Figure CN119018890A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and particularly relates to a modified biochar composite material and a preparation method and application thereof. The invention provides a preparation method of a modified biochar composite material, which comprises the following steps: mixing a biomass raw material and a pore-forming agent, and carrying out first calcination to obtain biochar; mixing the biochar, a nitrogen source and a cobalt source, and performing secondary calcination to obtain the modified biochar composite material. The preparation method provided by the invention is low in cost, and the obtained modified charcoal composite material has efficient catalytic performance as an ORR / OER electrocatalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and specifically relates to a modified biochar composite material and a preparation method and application thereof. Background Art

[0002] With the development of human society, the demand for energy is increasing day by day. However, excessive energy consumption has aroused human society's vigilance against environmental problems, such as environmental pollution and global warming, which have become more serious. Electrochemical energy conversion and storage technologies such as fuel cells and metal-air batteries have become a hot spot for development in the world's energy field due to their high energy density, economic benefits, environmental friendliness and excellent safety. Among them, oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) are the basic reactions of these technologies. However, the kinetics of these reactions are very slow, which hinders their commercial development.

[0003] At present, Pt is considered to be one of the most effective catalysts for oxygen reduction reaction (ORR), and Ir and Ru both show excellent performance as oxygen evolution reaction (OER) catalysts. The existing technology uses precious metal catalysts, which are expensive and have a single catalytic direction. For example, the Chinese patent with publication number CN111509240A uses precious metal platinum as an oxygen reduction reaction catalyst. Although precious metal catalysts have excellent performance, their high price, low reserves, and single catalytic direction hinder their large-scale commercial application in metal-air batteries. Summary of the invention

[0004] The object of the present invention is to provide a modified biochar composite material and a preparation method and application thereof. The preparation method provided by the present invention has low cost, and the obtained modified biochar composite material has efficient catalytic performance as an ORR / OER electrocatalyst.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a modified biochar composite material, comprising the following steps:

[0007] The biomass raw material and the pore-forming agent are mixed and first calcined to obtain biochar;

[0008] The biochar, nitrogen source and cobalt source are mixed and subjected to a second calcination to obtain the modified biochar composite material.

[0009] Preferably, the biomass raw material includes split wood; the particle size of the biomass raw material is ≤40 mesh;

[0010] The pore former includes potassium hydroxide;

[0011] The mass ratio of the biomass raw material to the pore-forming agent is 3.5-4.5:0.5-1.5.

[0012] Preferably, before mixing the biomass raw material and the pore-forming agent, the biomass raw material is also pretreated; the pretreatment includes: stirring and ultrasonically dispersing the biomass raw material and water, and then drying;

[0013] The stirring time is 3 to 7 minutes, and the ultrasonic dispersion time is 15 to 25 minutes;

[0014] The stirring and ultrasonic dispersion were repeated 3 times;

[0015] The drying temperature is 70-90°C.

[0016] Preferably, the temperature of the first calcination is 790-810° C., the heating rate to the first calcination temperature is 10° C. / min, and the holding time is 1.8-2.2 h; the first calcination is carried out under a protective atmosphere.

[0017] Preferably, after the first calcination, the obtained material is further acid-washed to neutrality and dried.

[0018] Preferably, the nitrogen source includes melamine and / or urea; the cobalt source includes cobalt chloride and / or cobalt nitrate;

[0019] The mass ratio of the biochar, the nitrogen source and the cobalt source is 0.4-0.6:4.5-5.5:0.1-0.5.

[0020] Preferably, the temperature of the second calcination is 790-810° C., the heating rate to the second calcination temperature is 10° C. / min, and the holding time is 80-100 min; the second calcination is carried out under a protective atmosphere.

[0021] The present invention also provides a modified biochar composite material prepared by the preparation method described in the above technical solution, comprising a nitrogen-doped biochar matrix and cobalt loaded in the nitrogen-doped biochar matrix.

[0022] The present invention also provides the use of the modified biochar composite material described in the above technical solution as an ORR / OER electrocatalyst.

[0023] The present invention provides a method for preparing a modified biochar composite material, comprising the following steps: mixing a biomass raw material and a pore-forming agent, performing a first calcination to obtain biochar; mixing the biochar, a nitrogen source and a cobalt source, performing a second calcination to obtain the modified biochar composite material. The present invention uses cobalt to modify nitrogen-doped biochar, wraps cobalt nanoparticles in the nitrogen-doped biochar, and forms a Co-N bond with N, so that the material has good electrical conductivity and promotes mass transfer of reactants, thereby improving ORR / OER activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The XRD diagrams of the modified biochar composite materials obtained in the examples and comparative examples;

[0025] Figure 2 This is a SEM image of the modified biochar composite material obtained in Example 2;

[0026] Figure 3 is the Raman graph of the modified biochar composite material obtained in Example;

[0027] Figure 4 TEM, HRTEM and EDS mapping images of the modified biochar composite material obtained in Example 2;

[0028] Figure 5 The XPS total spectrum and C1sXPS spectrum of the modified biochar composite material obtained in the embodiment and the comparative example;

[0029] Figure 6 The N1s and O1s XPS graphs of the modified biochar composite materials obtained in the examples and comparative examples;

[0030] Figure 7 The Co2p XPS graphs of the modified biochar composite materials obtained in the examples and comparative examples;

[0031] Figure 8 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the modified biochar composite material obtained in Example 2;

[0032] Fig. 9 ORR LSV diagrams of modified biochar composite materials obtained in Examples and Comparative Examples and commercially available Pt / C catalysts;

[0033] Fig.10 The ORRTafel diagrams of the modified biochar composite materials obtained in the examples and comparative examples and the commercially available Pt / C catalyst;

[0034] Fig.11 The half-wave potential diagrams of the modified biochar composite material obtained in the examples and comparative examples and the commercially available Pt / C catalyst;

[0035] Fig.12 The n value and yield diagram of the modified biochar composite material and the commercially available Pt / C catalyst obtained in Example 2;

[0036] Fig.13 The OER LSV diagrams of the modified biochar composite material obtained in the examples and comparative examples and the commercially available Ir / C catalyst;

[0037] Fig.14 The OER Tafel diagrams of the modified biochar composite material obtained in the examples and comparative examples and the commercially available Ir / C catalyst;

[0038] Fig.15 The overpotential diagrams of the modified biochar composite material obtained in the examples and comparative examples and the commercially available Ir / C catalyst;

[0039] Fig.16 The double-layer capacitance diagram of the modified biochar composite material obtained in the embodiment and the comparative example;

[0040] Fig.17 The electrochemical impedance spectroscopy of the modified biochar composite material obtained in the examples and comparative examples;

[0041] Fig.18 The LSV diagrams of the modified biochar composite materials obtained in the examples and comparative examples and the commercially available Pt / C+Ir / C catalyst;

[0042] Fig.19 It is a comparison chart of the potential difference between the modified biochar composite material obtained in the examples and comparative examples and the commercially available Pt / C+Ir / C catalyst. DETAILED DESCRIPTION

[0043] The present invention provides a method for preparing a modified biochar composite material, comprising the following steps:

[0044] The biomass raw material and the pore-forming agent are mixed and first calcined to obtain biochar;

[0045] The biochar, nitrogen source and cobalt source are mixed and subjected to a second calcination to obtain the modified biochar composite material.

[0046] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0047] The present invention mixes a biomass raw material and a pore-forming agent, performs a first calcination, and obtains biochar.

[0048] In the present invention, the biomass raw material preferably includes split wood; the particle size of the biomass raw material is preferably ≤40 mesh. In the present invention, the pore-forming agent preferably includes potassium hydroxide. In the present invention, the mass ratio of the biomass raw material to the pore-forming agent is preferably 3.5-4.5:0.5-1.5, and more preferably 4:1.

[0049] In the present invention, before mixing the biomass raw material and the pore-forming agent, the biomass raw material is preferably pretreated; the pretreatment preferably includes: stirring and ultrasonically dispersing the biomass raw material and water, and then drying; the stirring time is preferably 3 to 7 minutes, and more preferably 5 minutes; the ultrasonic dispersion time is preferably 15 to 25 minutes, and more preferably 20 minutes; the stirring and ultrasonic dispersion are repeated preferably 3 times; the drying temperature is preferably 70 to 90°C, and more preferably 80°C.

[0050] In the present invention, the temperature of the first calcination is preferably 790-810°C, more preferably 800°C; the heating rate to the first calcination temperature is preferably 10°C / min; the holding time is preferably 1.8-2.2h, more preferably 2h; the first calcination is carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen.

[0051] After the first calcination, the present invention preferably further comprises acid washing the obtained material to neutrality and drying; the reagent used for the acid washing is preferably 1 mol / L hydrochloric acid; the drying temperature is preferably 80°C.

[0052] After obtaining the biochar, the present invention mixes the biochar, a nitrogen source and a cobalt source, and performs a second calcination to obtain the modified biochar composite material.

[0053] In the present invention, the nitrogen source preferably includes melamine and / or urea; the cobalt source preferably includes cobalt chloride and / or cobalt nitrate; the cobalt chloride is preferably CoCl 2 6H 2 O; The mass ratio of the biochar, nitrogen source and cobalt source is preferably 0.4-0.6:4.5-5.5:0.1-0.5, more preferably 0.5:5.0:0.1-0.5, and further preferably 0.5:5.0:0.2-0.3.

[0054] In the present invention, the method of mixing the biochar, nitrogen source and cobalt source is preferably: adding water to the biochar, nitrogen source and cobalt source and heating and stirring until the water is completely evaporated; the temperature of the heating and stirring is preferably 80°C.

[0055] In the present invention, the temperature of the second calcination is preferably 790-810°C, more preferably 800°C; the heating rate to the second calcination temperature is preferably 10°C / min; the holding time is preferably 80-100min, more preferably 90min; the second calcination is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen.

[0056] The present invention also provides a modified biochar composite material prepared by the preparation method described in the above technical solution, comprising a nitrogen-doped biochar matrix and cobalt loaded in the nitrogen-doped biochar matrix.

[0057] In the present invention, the specific surface area of ​​the modified biochar composite material is preferably 290 to 440 m 2 ·g -1 In the present invention, the modified biochar composite material is preferably a mesoporous material.

[0058] The present invention also provides the use of the modified biochar composite material described in the above technical solution as an ORR / OER electrocatalyst. The present invention has no special limitation on the specific implementation of the application, and those familiar to those skilled in the art can be used.

[0059] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Example 1

[0061] Mix the wood with a particle size of ≤40 mesh and water, stir and disperse by ultrasonic, wherein the stirring time is 5 minutes and the ultrasonic dispersion time is 20 minutes, repeat 3 times, and then dry at 80°C;

[0062] The dried split wood and potassium hydroxide were mixed in a mass ratio of 4:1, and the mixture was heated to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere for calcination, and the mixture was kept warm for 2 hours; the calcined material was acid-washed with 1 mol / L hydrochloric acid until neutral, and dried at 80°C to obtain biochar;

[0063] Biochar, melamine and CoCl 2 6H 2O was mixed with water in a mass ratio of 0.5:5.0:0.1 for dispersion, and heated and stirred at 80°C until the water evaporated; the obtained mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere for calcination, and kept warm for 90 minutes to obtain the modified biochar composite material (denoted as CoN-DJC-0.1).

[0064] Example 2

[0065] A modified biochar composite material (denoted as CoN-DJC-0.3) was prepared in the manner of Example 1, wherein biochar, melamine and CoCl 2 6H 2 The mass ratio of O is 0.5:5.0:0.3.

[0066] Example 3

[0067] A modified biochar composite material (denoted as CoN-DJC-0.5) was prepared in the manner of Example 1, wherein biochar, melamine and CoCl 2 6H 2 The mass ratio of O is 0.5:5.0:0.5.

[0068] Comparative Example 1

[0069] A modified biochar composite material (denoted as N-DJC) was prepared in the same manner as in Example 1, except that CoCl 2 6H 2 O, that is, the mass ratio of biochar to melamine is 0.5:5.0.

[0070] Performance Testing

[0071] Test Example 1

[0072] The modified biochar composite materials obtained in the examples and comparative examples are characterized;

[0073] Figure 1 The XRD patterns of the modified biochar composite materials obtained in the examples and comparative examples are shown in Table 1. Figure 1 It can be seen that the diffraction peak at 26.32° corresponds to the (002) crystal plane of graphite carbon; there are two obvious diffraction peaks at 44.22° and 51.52°, corresponding to the (111) and (200) crystal planes of Co, respectively.

[0074] Figure 2 This is the SEM image of the modified biochar composite material obtained in Example 2. Figure 2 It can be seen that the modified biochar composite material provided by the present invention is mainly composed of carbon nano-helical tubes.

[0075] Figure 3The Raman diagram of the modified biochar composite material obtained in the example is Figure 3 It can be seen that 1354cm -1 and 1584cm -1 The two different characteristic peaks correspond to the D band and the G band. The D band represents the structural defects in the carbon lattice, and the G band represents the degree of graphitization. D / I G The intensity ratios of are 0.86, 0.64 and 0.55 respectively. This shows that the addition of Co increases the crystallinity of carbon and reduces the lattice defects of carbon. High graphitization is the key to conductivity, and abundant defect sites lead to more oxygen electrocatalytic active centers. While moderate I D / I G The value is more favorable for the catalytic reaction.

[0076] Figure 4 TEM, HRTEM and EDS mapping images of the modified biochar composite material obtained in Example 2. Transmission electron microscopy (TEM) shows that the metal nanoparticles Co are well encapsulated in the carbon framework. Co nanoparticles are distributed inside the carbon nanotubes. Coating Co species in carbon nanotubes can effectively prevent the aggregation and dissolution of Co species, and improve the stability and life of the entire catalyst. Co nanoparticles are distributed inside and on the surface of carbon nanotubes. Coating Co species in carbon nanotubes can effectively prevent the aggregation and dissolution of Co species, and improve the stability and life of the entire catalyst. High-resolution transmission electron microscopy (HRTEM) images show that the lattice distances of Co particles are 0.177 and 0.205 nm, corresponding to the (200) and (111) crystal planes of Co, respectively. EDS images show that the Co, N, O and C elements in Example 2 are uniformly distributed.

[0077] Figures 5 to 7 The XPS graphs of the modified biochar composite materials obtained in the examples and comparative examples are shown in FIG. Figure 5 is the XPS total spectrum and C1s graph, Figure 6 is the N1s and O1s diagram, Figure 7It is a Co2p diagram. The XPS spectra of Example 1, Example 2, Example 3 and the comparative example show the presence of C, N, O and Co elements. The XPS spectrum of C1s shows three peaks at 284.7, 285.1 and 293.2 eV, which correspond to C=C, CC / CN and C=O, respectively. The high-resolution N1s spectrum shows five N substances, represented by nitrogen oxide (406.4 eV), NO (405.0 eV), graphitic nitrogen (402.9 eV), pyrrolic nitrogen (401.3 eV) and pyridinic nitrogen (398.5 eV). Pyridinic nitrogen increases the starting potential of the redox reaction, and graphitic nitrogen determines the diffusion limiting current of the redox reaction. The XPS spectrum of O1s shows two peaks at 531.5 and 532.5 eV, which correspond to MO and M-OH, respectively. The high-resolution Co 2p spectrum is divided into eight peaks. The peaks at 778.6 and 793.3 eV correspond to Co 0 2p 3 / 2 and Co 0 2p 1 / 2 The peaks at 779.8 and 795.2 eV correspond to Co 3+ 2p 3 / 2 and Co 3+ 2p 1 / 2 At 781.7eV (Co 2+ 2p 3 / 2 ) and 797.2eV(Co 2+ 2p 1 / 2 The two peaks at 786.6 and 802.8 eV are satellite peaks.

[0078] Figure 8 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the modified biochar composite material obtained in Example 2. The isotherm curve of Example 2 shows a typical type IV curve and an H3 type hysteresis loop, indicating that the obtained catalyst has mesopores. The specific surface area of ​​Example 2 can reach 334.76m 2 ·g -1 , catalysts with large specific surface areas can provide more active sites, which can promote the transfer of reactants and increase the redox reaction rate.

[0079] Test Example 2

[0080] The ORR performance of the modified biochar composite material obtained in the embodiment and the comparative example was tested in an oxygen-saturated 0.1M KOH solution at a rotation speed of 1600 rpm. The test results are shown in FIG. Figures 9 to 12 As shown;

[0081] Fig. 9 The ORR LSV diagrams of the modified biochar composite material and the commercially available Pt / C catalyst obtained in the examples and comparative examples are shown in Table 1. Fig. 9 It can be seen that the half-wave potentials of Example 1, Example 2, Example 3 and Comparative Example 1 are 0.78 V, 0.83 V, 0.79 V and 0.72 V, respectively, and the half-wave potential of Example 2 is the same as that of the commercial electrocatalyst Pt / C.

[0082] Fig.10 The ORRTafel diagrams of the modified biochar composite material and the commercially available Pt / C catalyst obtained in the examples and comparative examples are shown in Table 1. Fig.10 It can be seen that the ORR Tafel slopes of Example 1, Example 2, Example 3 and Comparative Example 1 are 86 mV·dec respectively. -1 、59mV·dec -1 、79mV·dec -1 and 95mV·dec -1 The Tafel slope of Example 2 is better than that of the commercial electrocatalyst Pt / C (74 mV·dec -1 ). A low Tafel slope indicates that the catalyst has excellent ORR kinetics.

[0083] Fig.11 The half-wave potential diagrams of the modified biochar composite material and the commercially available Pt / C catalyst obtained in the examples and comparative examples are shown in Table 1. Fig.11 It can be seen that the half-wave potentials of Example 1, Example 2, Example 3, Comparative Example 1 and the commercially available Pt / C catalyst are 0.78 V, 0.83 V, 0.79 V, 0.72 V and 0.83 V, respectively.

[0084] Fig.12 The n value and yield diagram of the modified biochar composite material and the commercially available Pt / C catalyst obtained in Example 2 are shown in FIG. Fig.12 It can be seen that the electron transfer number n is close to 4, H 2 O 2 The yield remained below 10%, indicating that the reaction belongs to a four-electron reduction mechanism.

[0085] Test Example 3

[0086] The OER performance of the modified biochar composite material obtained in the embodiment and the comparative example was tested in a 1M KOH electrolyte using a three-electrode system. The test results are shown in FIG. Figures 13 to 19 As shown;

[0087] Fig.13 The OER LSV diagrams of the modified biochar composite material and the commercially available Ir / C catalyst obtained in the examples and comparative examples are shown in Table 1. Fig.13It can be seen that the materials of Example 1, Example 2, Example 3 and Comparative Example 1 have a current density of 10 mA·cm -2 The overpotentials at the time of the reaction were 1.60 V, 1.52 V, 1.59 V and 1.71 V respectively. The overpotentials at the time of the reaction of Example 2 were 10 mA cm -2 The overpotential at this time is slightly better than that of the commercial electrocatalyst Ir / C (1.53 V).

[0088] Fig.14 The OER Tafel diagrams of the modified biochar composite material and the commercially available Ir / C catalyst obtained in the examples and comparative examples are shown in Table 1. Fig.14 It can be seen that the OER Tafel slopes of Example 1, Example 2, Example 3 and Comparative Example 1 are 241 mV·dec respectively. -1 、111mV·dec -1 、209mV·dec -1 and 374mV·dec -1 The Tafel slope of Example 2 is better than that of the commercial electrocatalyst Ir / C (124 mV·dec -1 ) is the Tafel slope of .

[0089] Fig.15 The overpotential diagrams of the modified biochar composite material and the commercially available Ir / C catalyst obtained in the examples and comparative examples are shown in FIG. Fig.15 It can be seen that the catalysts of Example 1, Example 2, Example 3, Comparative Example 1 and the commercially available Ir / C have a high current density of 10 mA·cm -2 The overpotentials are 1.60V, 1.52V, 1.59V, 1.71V and 1.53V respectively.

[0090] Fig.16 The double-layer capacitance diagram of the modified biochar composite material obtained in the examples and comparative examples is shown in FIG. Fig.16 It can be seen that the C calculated from the CV curves (support material) of the catalysts of Example 1, Example 2, Example 3 and Comparative Example 1 dl The values ​​are 42.16mF·cm -2 、45.12mF·cm -2 、20.57mF·cm -2 、14.26mF·cm -2 , Example 2 has a higher electrochemical surface area (ECSA).

[0091] Fig.17 The electrochemical impedance spectroscopy of the modified biochar composite material obtained in the examples and comparative examples is shown in FIG. Fig.17It can be seen that the electrochemical impedance spectroscopy (EIS) of Example 2 shows a smaller charge transfer resistance, indicating that Example 2 has better electron transfer ability and higher OER activity than Example 1 and Example 3.

[0092] Fig.18 The LSV diagrams of the modified biochar composite materials obtained in the examples and comparative examples and the commercially available Pt / C+Ir / C catalysts are shown in Figure 2. j=10mA·cm -2 E with ORR 1 / 2 The potential difference between j=10mA·cm -2 -E 1 / 2 ), and the ORR / OER activity of the catalyst was evaluated. The figure shows the LSV curve of ORR / OER. It can be obtained that ΔE=0.82V of Example 1, ΔE=0.69V of Example 2, ΔE=0.80V of Example 3, ΔE=0.99V of Comparative Example 1, and ΔE=0.70V of commercially available Pt / C+Ir / C.

[0093] Fig.19 The potential difference comparison diagram of the modified biochar composite material obtained in the embodiment and the comparative example and the commercially available Pt / C+Ir / C catalyst is shown; it can be obtained that ΔE=0.82V of embodiment 1, ΔE=0.69V of embodiment 2, ΔE=0.80V of embodiment 3, ΔE=0.99V of comparative example 1 and ΔE=0.70V of commercially available Pt / C+Ir / C. The ORR / OER of the embodiment is slightly better than that of commercially available Pt / C+Ir / C.

[0094] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a modified biochar composite material, characterized in that: The following steps are involved: The biomass raw material and the pore-forming agent are mixed and first calcined to obtain biochar; The biochar, nitrogen source and cobalt source are mixed and subjected to a second calcination to obtain the modified biochar composite material.

2. The preparation method according to claim 1, characterized in that: The biomass raw material includes split wood; the particle size of the biomass raw material is ≤40 mesh; The pore former includes potassium hydroxide; The mass ratio of the biomass raw material to the pore-forming agent is 3.5-4.5:0.5-1.

5.

3. The preparation method according to claim 2, characterized in that: Before mixing the biomass raw material and the pore-forming agent, the biomass raw material is pretreated; the pretreatment includes: stirring and ultrasonically dispersing the biomass raw material and water, and then drying; The stirring time is 3 to 7 minutes, and the ultrasonic dispersion time is 15 to 25 minutes; The stirring and ultrasonic dispersion were repeated 3 times; The drying temperature is 70-90°C.

4. The preparation method according to claim 2 or 3, characterized in that: The temperature of the first calcination is 790-810° C., the heating rate to the first calcination temperature is 10° C. / min, and the holding time is 1.8-2.2 h; the first calcination is carried out under a protective atmosphere.

5. The preparation method according to claim 4, characterized in that: After the first calcination, the obtained material is acid washed to neutrality and dried.

6. The preparation method according to claim 1, characterized in that: The nitrogen source includes melamine and / or urea; the cobalt source includes cobalt chloride and / or cobalt nitrate; The mass ratio of the biochar, the nitrogen source and the cobalt source is 0.4-0.6:4.5-5.5:0.1-0.

5.

7. The preparation method according to claim 1 or 6, characterized in that: The temperature of the second calcination is 790-810° C., the heating rate to the second calcination temperature is 10° C. / min, and the holding time is 80-100 min; the second calcination is carried out under a protective atmosphere.

8. The modified biochar composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The invention comprises a nitrogen-doped biochar matrix and cobalt loaded in the nitrogen-doped biochar matrix.

9. Use of the modified biochar composite material according to claim 8 as an ORR / OER electrocatalyst.

Citation Information

Patent Citations

  • Active carbon-loaded nitrogen-doped cobalt catalyst and preparation method and application thereof

    CN104383953A

  • Preparation method of cobalt nitrogen co-doped biomass carbon oxidation reduction catalyst

    CN109174157A

Cited By

  • Modified carbonized bamboo composite material and preparation method and application thereof

    CN119833652A