Method for preparing activated carbon by taking crop straw as raw material and application of activated carbon

Through the coordinated activation and desilication of phosphoric acid, zinc chloride, and aminoindole hydrochloride, the problem of difficult to improve the porosity and specific surface area of ​​crop straw activated carbon was solved, and activated carbon with high adsorption performance was prepared, which solved the collapse of the pore structure and the problem of degraded adsorption performance, the efficient adsorption effect of organic solvents is achieved.

CN119018891AActive Publication Date: 2024-11-26FUJIAN XINSEN CARBON

Patent Information

Application Number
CN202411127074.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the prior art, when using crop straw to prepare activated carbon, the porosity and specific surface area are difficult to improve, and the pore structure collapses due to excessive activation, affecting the adsorption performance.

Method used

The co-activation method of phosphoric acid, zinc chloride, and aminoindole hydrochloride was adopted, and the crop straw was desilicate before activation, and pre-activated and carbonized through specific impregnation liquid ratios and conditions to prepare rich and Stable pores and high specific surface area activated carbon.

Benefits of technology

The prepared activated carbon has excellent adsorption performance, with high first adsorption value and the adsorption value retention rate after 30 adsorption-desorption cycles is above 90%, which significantly improves the adsorption performance of activated carbon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018891A_ABST
    Figure CN119018891A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing activated carbon by taking crop straw as a raw material, which comprises the following steps: (S1) pretreatment: sequentially crushing, washing and drying the crop straw to obtain a pretreated material; (S2) desiliconization treatment: putting the pretreated material into a hydrofluoric acid solution for heat treatment, cleaning to be neutral, and drying to obtain a desiliconized material; (S3) pre-activation: putting the desiliconized material into an impregnation liquid, performing impregnation activation at 80-110 DEG C in a closed state, and then performing granulation and drying to obtain prefabricated activated carbon; the impregnation liquid is a mixed aqueous solution prepared from phosphoric acid, zinc chloride and aminoindole hydrochloride according to the mass ratio of 1: (0.15-0.3): (0.1-0.25); and (S4) carbonization: carbonizing the prefabricated activated carbon in an inert atmosphere to obtain the activated carbon. The prepared activated carbon has excellent adsorbability to organic solvents, the first adsorption value is high, and the retention rate of the adsorption value after 30 times of adsorption-desorption cycles is 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of activated carbon preparation, and particularly relates to a method for preparing activated carbon using crop straw as raw material and application of the method in solvent recovery. Background Art

[0002] Activated carbon is widely used in the field of solvent recovery, and its adsorption performance is closely related to the characteristics of the pore structure. Solvent recovery activated carbon generally refers to activated carbon used for organic solvent recovery, mainly used for high-end air purification or various gas solvent recovery. At present, coal-based granular carbon and wood-based activated carbon are mostly used, but coal is a non-renewable resource. At the same time, at the same production cost, the technical indicators of wood-based activated carbon are better than those of coal-based carbon, so the demand for wood-based activated carbon is growing. At present, the production of wood-based activated carbon mainly uses trees as raw materials, but trees grow very slowly, and cutting trees for charcoal burning seriously damages the ecological environment. my country has abundant crop straw resources, but most of them are left in the fields or burned in the open air, which not only causes a waste of resources, but also leads to serious environmental pollution. In order to alleviate the contradiction between the demand for wood-based activated carbon and the protection of ecological resources, it is of great significance to use crop straw to prepare activated carbon.

[0003] Traditionally, activated carbon prepared from crop straw is activated by phosphoric acid, but the reaction cycle is long, the efficiency is low, and the porosity needs to be further improved. The main reason is that crop straw has high internal binding force and dense structure, and cellulose, hemicellulose and lignin are entangled and restricted with each other, so its structure is stable and not easily destroyed. If CO2 and H2O atmosphere activation are combined with phosphoric acid activation, the activation efficiency can be improved, the porosity and specific surface area can be increased, but it is easy to cause over-activation, which leads to the collapse of the pore structure and the decline of adsorption performance. Chinese patent CN 117208901A discloses a honeycomb solvent recovery activated carbon and its preparation method, the preparation method comprises the following steps: S1, take bamboo, wash, dry and sterilize to obtain clean raw materials; S2, add carbon body after heating, start vacuum pump to control pressure, keep heat and pressure, cool to room temperature and crush, and spray with acid solution at the same time, after solid-liquid separation, obtain mixed material; S3, ball mill into powder, sieve the mixed material after ball milling to obtain mixed powder; S4, add acid solution to mix and stir, activate under water vapor atmosphere, cool to obtain activated product; S5, wash, filter, take solid and dry to obtain activated carbon. Although the water vapor atmosphere used in this invention is conducive to the formation of activated carbon mesopores in the process of phosphoric acid activation of bamboo, microporous activated carbon must be added in step S2 to overcome the defects of pore structure collapse and yield reduction caused by over-activation. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to provide a method for preparing activated carbon using crop straw as raw material, through the synergistic activation of phosphoric acid, zinc chloride, and aminoindole hydrochloride and desiliconization of crop straw before activation, to prepare activated carbon with rich and stable pores and high specific surface area, and the activated carbon has excellent adsorption capacity for organic solvents.

[0005] A method for preparing activated carbon using crop straw as raw material comprises the following steps:

[0006] (S1) pretreatment: crushing, washing and drying the crop straw in sequence to obtain a pretreated material;

[0007] (S2) Desiliconization treatment: placing the pretreated material in a hydrofluoric acid solution for heat treatment, cooling, washing until neutral, and drying to obtain a desiliconized material;

[0008] (S3) pre-activation: placing the desiliconized material in an impregnation solution, impregnating and activating it at 80-110° C. in a closed state, and then granulating and drying it in sequence to obtain prefabricated activated carbon; the impregnation solution is a mixed aqueous solution of phosphoric acid, zinc chloride, and aminoindole hydrochloride prepared in a mass ratio of 1: (0.15-0.3): (0.1-0.25);

[0009] (S4) Carbonization: The prefabricated activated carbon is carbonized, cooled, washed, and dried under an inert atmosphere to obtain activated carbon.

[0010] The invention prepares activated carbon by pre-activating crop straw after desiliconization with a high-activity impregnation solution formed by phosphoric acid, zinc chloride and aminoindole hydrochloride and then carbonizing the crop straw; the prepared activated carbon has a high specific surface area, stable and abundant pores. Phosphoric acid is a Lewis acid, which can accelerate the decomposition of cellulose and hemicellulose in crop straw and promote the aromatic condensation reaction in the process of cellulose carbonization; zinc chloride has a strong catalytic dehydroxylation and dehydration effect, so that hydrogen and oxygen in the raw material escape in the form of water vapor, thereby inhibiting the generation of tar and avoiding pore blockage. Aminoindole hydrochloride is a chloride salt containing a benzene ring and a nitrogen heterocycle. The inventors have found that aminoindole hydrochloride can synergistically activate crop straw with phosphoric acid and zinc chloride, so that the prepared activated carbon has more abundant pores and a higher specific surface area. The possible reason is that, on the one hand, the benzene ring and nitrogen heterocycle in aminoindole hydrochloride interact with the benzene ring in biomass, thereby promoting phosphoric acid and zinc chloride to activate the crop straw; on the other hand, there are a large number of hydroxyl groups on the cellulose molecular chain in the crop straw, and there are strong hydrogen bonds between or within the cellulose molecules, and aminoindole hydrochloride can form hydrogen bonds with the hydroxyl groups on the cellulose molecular chain, thereby weakening the hydrogen bonds between or within the cellulose molecules and increasing the spatial volume of cellulose, thereby making the cellulose loose. The present invention prepares high-performance activated carbon through the synergistic effect of phosphoric acid, zinc chloride and aminoindole hydrochloride, but the three cannot be combined in any proportion; if the content of zinc chloride is too low, the effect of zinc chloride is limited, but when the content is too high, it will block the formed pores; if the content of aminoindole hydrochloride is too low, the effect of aminoindole hydrochloride is also limited, but when the content is too high, the phosphoric acid content will be low, thereby reducing the effect of activation and pore formation; therefore, the ratio of the three needs to be controlled within an appropriate range to exert the synergistic effect.

[0011] In addition, the silicon dioxide contained on the surface of the crop straw will hinder the contact between phosphoric acid, zinc chloride, aminoindole hydrochloride and the fiber and the activation reaction, thereby hindering the generation and development of pores in the activated carbon; the present invention desiliconizes the crop straw before carbonization and activation, and the desiliconization treatment will leave pores at the original position of the silicon dioxide, and the pores will be extended and expanded in the subsequent carbonization and activation process.

[0012] Furthermore, the crop straw in step (S1) is one or more of corn straw, wheat straw, rice straw, and soybean straw; the crushing is crushing to 100-400 mesh, and the crushing method is air flow crushing, high-speed crushing or ball milling; the drying is drying at 80-100° C. for 24-36 hours.

[0013] Furthermore, in step (S2), the concentration of the hydrofluoric acid solution is 5-10wt%, the solid-liquid ratio of the pre-treated material to the hydrofluoric acid solution is 1kg:1-3L; the heat treatment condition is: 50-70°C for 30-90min. The use of hydrofluoric acid heat treatment can not only remove the silicon-containing harmful components in the crop straw raw material, but also further dissolve the non-cellulose components in the crop straw, reducing the resistance of subsequent high-temperature carbonization.

[0014] Furthermore, the aminoindole hydrochloride in step (S3) is at least one of 5-aminoindole hydrochloride, 4-aminoindole hydrochloride, 3-aminoindole hydrochloride, 2-aminoindole hydrochloride, 3-(2-aminoethyl)indole hydrochloride, and 3-(2-aminopropyl)indole hydrochloride.

[0015] Furthermore, in step (S3), the mass ratio of phosphoric acid, zinc chloride and aminoindole hydrochloride in the impregnation solution is 1:(0.2-0.25):(0.15-0.2).

[0016] Furthermore, in step (S3), the concentration of the impregnation liquid is 50-75wt%; the solid-liquid ratio of the desiliconized material to the impregnation liquid is 1kg:1-3L; and the impregnation activation is performed for 1.5-3h.

[0017] In step (S3), the 80-110°C is the temperature for immersion activation, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C.

[0018] Furthermore, the granulation in step (S3) is to obtain columnar or spherical granules through a granulator, for example, through a plunger granulator, cut into rods or strips with a diameter of 2 to 5 mm, such as 2 mm, 3 mm, 4 mm, and a length of 5 to 8 mm; through a needle granulator, spherical particles are formed, and the particle size can be 1.5 mm, 2 mm, 2.5 mm, 3 mm; the drying is drying in an oven at 100 to 150° C. for 24 to 36 hours.

[0019] Furthermore, in step (S4), the inert atmosphere is nitrogen, argon or helium; the carbonization conditions are: heating to 500-700°C at a heating rate of 3-8°C / min in a rotary kiln, keeping warm for 2-5h, and the rotary kiln speed is 15-20rpm; the washing is boiling in water for 30-60min to remove residual phosphoric acid in the carbonized material, so that the phosphoric acid in the carbonized material is less than 200ppm, and the residual phosphoric acid can also be recovered for use in step (S1); the drying is drying to a moisture content of <5wt%, such as baking in an oven at 100-150°C for 24-36h.

[0020] In a second aspect, the present invention provides activated carbon prepared by the above method for preparing activated carbon.

[0021] In a third aspect, the present invention provides the use of activated carbon prepared by the above method for preparing activated carbon in solvent recovery.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention prepares porous activated carbon by impregnating and activating crop straw after desiliconization with a high-activity impregnation solution formed by phosphoric acid, zinc chloride and aminoindole hydrochloride in a specific mass ratio and then carbonizing the impregnation solution; the prepared activated carbon has abundant and stable pores and a high specific surface area, and has excellent adsorption for organic solvents, and not only has a high first adsorption value, but also the adsorption value retention rate after 30 adsorption-desorption cycles is above 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the SEM image of the prepared activated carbon. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with specific embodiments. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight, and the reagents used are all commercially available reagents in the art.

[0026] Example 1

[0027] (S1) Pretreatment: The wheat straw is pneumatically crushed to 200 mesh, washed twice with water, and then placed in an oven for drying at 90° C. for 24 h to obtain a pretreated material;

[0028] (S2) Desiliconization treatment: the pretreated material is placed in a hydrofluoric acid solution with a concentration of 5 wt% at a solid-liquid ratio of 1 kg:2 L, treated at 60° C. for 60 min, then cooled, washed with pure water until neutral, and dried to obtain a desiliconized material;

[0029] (S3) Preactivation: first, phosphoric acid, zinc chloride, and 4-aminoindole hydrochloride are prepared into a mixed aqueous solution with a concentration of 60 wt % according to a mass ratio of 1:0.15:0.1, i.e., an impregnation solution; then, the desiliconized material is placed in the impregnation solution according to a solid-liquid ratio of 1kg:2L, and impregnated and activated in a kneader at 100°C for 2h to obtain a kneaded material; then, the kneaded material is formed into strip particles with a particle size of 3mm and a length of 7mm by a plunger granulator, and dried in an oven at 100°C for 36h to obtain a prefabricated material;

[0030] (S4) Carbonization: The preform was placed in a rotary kiln, heated to 600°C at a heating rate of 6°C / min under a nitrogen atmosphere, and kept warm for 2.5 hours at a rotary kiln speed of 20 rpm; after carbonization, it was naturally cooled to room temperature, boiled in water for 40 minutes, and baked in an oven at 120°C for 24 hours to obtain activated carbon.

[0031] The SEM image of the activated carbon prepared is as follows Figure 1 shown.

[0032] Example 2

[0033] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.15:0.15.

[0034] Example 3

[0035] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.2:0.15.

[0036] Example 4

[0037] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.25:0.2.

[0038] Example 5

[0039] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.3:0.25.

[0040] Example 6

[0041] The rest is the same as Example 1, except that 3-(2-aminoethyl)indole hydrochloride is used instead of 4-aminoindole hydrochloride in step (S3).

[0042] Example 7

[0043] The rest is the same as Example 1, except that rice straw is used instead of wheat straw in step (S1).

[0044] Comparative Example 1

[0045] The rest is the same as Example 1, except that the impregnation solution in step (S3) is an aqueous solution of phosphoric acid and zinc chloride in a mass ratio of 1:0.15, that is, it does not contain 4-aminoindole hydrochloride.

[0046] Comparative Example 2

[0047] The rest is the same as Example 1, except that the impregnation solution in step (S3) is an aqueous solution of phosphoric acid and 4-aminoindole hydrochloride in a mass ratio of 1:0.1, that is, it does not contain zinc chloride.

[0048] Comparative Example 3

[0049] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.4:0.3.

[0050] Comparative Example 4

[0051] The rest is the same as Example 1, except that the mass ratio of phosphoric acid, zinc chloride and 4-aminoindole hydrochloride in the impregnation solution of step (S3) is 1:0.1:0.05.

[0052] Comparative Example 5

[0053] The rest is the same as Example 1, except that step (S2) is omitted, that is, the crop straw is not subjected to desiliconization treatment.

[0054] Testing and analysis

[0055] 1) Specific surface area determination: A low-temperature nitrogen adsorption experiment was performed on the activated carbons prepared in the examples and comparative examples using a Tristar II 3020 fully automatic specific surface analyzer produced by Micromeritics Instrument Corporation of the United States to determine the specific surface area of ​​the activated carbons.

[0056] 2) Adsorption performance test:

[0057] According to GB / T 12496.8-1999, the iodine adsorption values ​​of the activated carbons prepared in the examples and comparative examples were measured;

[0058] The toluene adsorption value of the activated carbon prepared in the example and the comparative example was determined according to GB / T 35815-2018.

[0059] 3) Adsorption performance retention rate test: After the activated carbon prepared in the embodiment and the comparative example was subjected to 30 toluene adsorption-desorption cycles (100°C water vapor desorption for 60 min), its iodine adsorption value and toluene adsorption value were tested again, and compared with the first test value, the adsorption value retention rate was calculated.

[0060]

[0061] Table 1 Specific surface area and adsorption performance test

[0062]

[0063]

[0064] As can be seen from Table 1, the activated carbon prepared in Examples 1 to 7 of the present invention has a higher specific surface area, and its first iodine adsorption value is more than 1200 mg / g, and its first toluene adsorption value is 300 mg / g, which are significantly higher than the comparative example; and the iodine adsorption value retention rate and toluene adsorption value retention rate after 30 adsorption-desorption cycles are both above 90%.

[0065] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the adsorption effect of the prepared activated carbon is significantly reduced due to the lack of aminoindole hydrochloride or zinc chloride in the impregnation solution.

[0066] Comparison of Example 1 with Comparative Examples 2 and 3 shows that the synergistic effect can be effectively exerted only when the mass ratio of phosphoric acid, zinc chloride and aminoindole hydrochloride is controlled within an appropriate range.

[0067] By comparing Example 1 with Comparative Example 4, it can be seen that desiliconization of crop straw is beneficial to the increase of specific surface area, which means that it is beneficial to the formation of abundant pores, thereby improving the adsorption effect.

[0068] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A method for preparing activated carbon using crop straw as raw material, characterized in that: The following steps are involved: (S1) pretreatment: crushing, washing and drying the crop straw in sequence to obtain a pretreated material; (S2) Desiliconization treatment: placing the pretreated material in a hydrofluoric acid solution for heat treatment, cooling, washing until neutral, and drying to obtain a desiliconized material; (S3) pre-activation: placing the desiliconized material in an impregnation solution, impregnating and activating it at 80-110° C. in a closed state, and then granulating and drying it in sequence to obtain prefabricated activated carbon; the impregnation solution is a mixed aqueous solution of phosphoric acid, zinc chloride, and aminoindole hydrochloride prepared in a mass ratio of 1: (0.15-0.3): (0.1-0.25); (S4) Carbonization: The prefabricated activated carbon is carbonized, cooled, washed, and dried under an inert atmosphere to obtain activated carbon.

2. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: In step (S1), the crop straw is one or more of corn straw, wheat straw, rice straw, and soybean straw; the crushing is crushing to 100-400 meshes, and the crushing method is air flow crushing, high-speed crushing or ball milling; and the drying is drying at 80-100° C. for 24-36 hours.

3. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: In step (S2), the concentration of the hydrofluoric acid solution is 5-10wt%, and the solid-liquid ratio of the pretreated material to the hydrofluoric acid solution is 1kg:1-3L; the heat treatment conditions are: 50-70°C for 30-90min.

4. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: The aminoindole hydrochloride in step (S3) is at least one of 5-aminoindole hydrochloride, 4-aminoindole hydrochloride, 3-aminoindole hydrochloride, 2-aminoindole hydrochloride, 3-(2-aminoethyl)indole hydrochloride, and 3-(2-aminopropyl)indole hydrochloride.

5. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: In step (S3), the mass ratio of phosphoric acid, zinc chloride and aminoindole hydrochloride in the impregnation solution is 1: (0.2-0.25): (0.15-0.2).

6. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: In step (S3), the concentration of the impregnation liquid is 50-75wt%; the solid-liquid ratio of the desiliconized material to the impregnation liquid is 1kg:1-3L; and the impregnation activation is performed for 1.5-3h.

7. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: The granulation in step (S3) is to obtain columnar or spherical granules by a granulator; and the drying is to dry in an oven at 100-150° C. for 24-36 hours.

8. The method for preparing activated carbon using crop straw as raw material according to claim 1, characterized in that: In step (S4), the inert atmosphere is nitrogen, argon or helium; the carbonization conditions are: heating to 500-700°C at a heating rate of 3-8°C / min in a rotary kiln, keeping warm for 2-5h, and the rotary kiln speed is 15-20rpm; the washing is boiling in water for 30-60min; the drying is drying to a moisture content of <5wt%, such as baking in an oven at 100-150°C for 24-36h.

9. Activated carbon prepared by the method for preparing activated carbon according to any one of claims 1 to 8.

10. Use of the activated carbon prepared by the method for preparing activated carbon according to any one of claims 1 to 8 in solvent recovery.

Citation Information

Patent Citations

  • Organic fertilizer carrier prepared from carbonized rice hull granules and preparation method thereof

    CN106588435A

  • Biomass-based porous carbon and preparation method thereof

    CN116924396A

  • Low-ash-content activated carbon with crop straw as raw material and preparation method of low-ash-content activated carbon

    CN117049536A

  • Computerized systems and methods for decision-based delivery consolidation

    KR102432598B1

  • Carbon material for polarizable electrodes and method for producing same

    US20150287545A1

Cited By

  • Preparation method of biomass carbonized material with low silicon and aluminum content

    CN121405069A

  • Preparation method of lotus seedpod-based activated carbon with improved low-temperature adsorbability

    CN121553940A

  • A method for preparing lotus seedpod shell-based activated carbon with improved low-temperature adsorption properties

    CN121553940B