Preparation method of precipitated white carbon black for new energy automobile tire
Through step-by-step reaction and emulsifying hydrogen-containing silicone oil treatment, combined with specific overacid aging steps, the problem of insufficient dispersion of white carbon black in new energy vehicle tires is solved, and the effects of high dispersion, low rolling resistance and high grip are achieved. Suitable for mass production and reduces costs.
Patent Information
- Application Number
- CN202411175580.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing precipitation method of white carbon black preparation cannot meet the requirements of high dispersion, low rolling resistance, high grip and stability of new energy vehicle tires, and has high production efficiency and cost.
The acid-base co-flow reaction method of controlling particle size and structure is adopted in step-by-step reaction, combined with emulsified hydrogen-containing silicone oil and specific peracid aging treatment, adjust the generation rate and particle size distribution of white carbon black, improve its dispersion in rubber and performance.
It significantly improves the dispersion and performance of white carbon black, reduces the rolling resistance of tires, improves grip, meets the performance requirements of new energy vehicle tires, and simplifies the production process, reduces costs, and is suitable for large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precipitated silica production methods, and in particular to a method for preparing precipitated silica for new energy vehicle tires. Technical Background
[0002] With the rapid development of new energy vehicles, the performance requirements of their supporting tires are getting higher and higher. New energy vehicle tires not only require lower rolling resistance to significantly increase the mileage and meet people's needs for long-distance travel, but also need to have better grip to ensure driving safety, especially under high-speed driving and complex road conditions. As a key filler for rubber tires, the performance of white carbon black directly affects the quality of the tire. At present, the most prominent quality problem of white carbon black is insufficient dispersion, because in rubber, the poor dispersion of white carbon black will lead to its inability to fully play its reinforcing role, which in turn affects the performance of the tire. Specifically, it is difficult to reduce the rolling resistance of the tire to an ideal level, which will not only increase energy consumption and reduce mileage, but also contradict the concept of energy conservation and environmental protection of new energy vehicles; second, the grip is also difficult to be effectively improved, affecting driving safety; third, it leads to a decrease in the wear resistance and aging resistance of the tire, shortening the service life of the tire.
[0003] At present, precipitation method is one of the common methods for preparing silica, but the existing method for preparing silica by precipitation method for new energy vehicle tires has many limitations:
[0004] CN103435051B discloses a process for producing highly dispersed silica for green tires. However, due to the large difference in reaction temperature between the first step and the second step, the product particle size range is wide, resulting in poor dispersion performance of the obtained silica product, which cannot meet the requirements of green tires for highly dispersed silica.
[0005] CN115321548A discloses a method for preparing highly dispersed white carbon black for new energy vehicle tires. The precipitated silica obtained still needs to be modified before it can be used as a tire reinforcement material. The product quality stability is poor and the expected performance cannot be achieved after the tire is reinforced.
[0006] CN113905985A discloses a precipitated silica for green tires and a preparation method thereof. The precipitated silica adopts staged solid-liquid separation, has a complex preparation process, and requires precise control of the pH value of each stage. It has high requirements for equipment and personnel, increases production difficulty and cost, leads to reduced production efficiency, and is not conducive to large-scale production.
[0007] Therefore, it is necessary to develop a method for preparing precipitated silica suitable for new energy vehicle tires to overcome the defects of the prior art and prepare silica with good dispersibility, excellent performance, good stability, low cost and high production efficiency to meet the requirements of new energy vehicle tires for low rolling resistance and high grip.
[0008] The quality index requirements for silica used in new energy vehicle tires are as follows:
[0009] Dispersion: It has good dispersibility, with a dispersion of not less than 9.5, so that it can more easily combine with rubber molecules when mixed with rubber, ensuring good dispersion effect to improve the performance of the rubber after mixing.
[0010] Rolling resistance: It can effectively reduce the rolling resistance of tires. Compared with ordinary tires, the rolling resistance is required to be reduced by 10-20%, thereby achieving an energy saving effect of 2%-4%.
[0011] Grip: Excellent grip ensures that the tires can provide reliable traction and handling stability under various road conditions.
[0012] Other properties: Can significantly improve the physical properties of rubber, enhance the tensile strength of rubber, etc. Summary of the invention
[0013] The purpose of the present invention is to provide a method for preparing precipitated silica for new energy vehicle tires with good dispersibility, stable performance, low cost and high production efficiency, so as to meet the requirements of new energy vehicle tires for low rolling resistance and high grip.
[0014] To achieve the above purpose, the preparation method of precipitated silica for new energy vehicle tires of the present invention comprises the following steps:
[0015] S1. Preparation of acid-base co-current reaction materials: Add tap water and emulsified hydrogenated silicone oil as base liquid into the reactor, with a mass ratio of tap water: emulsified hydrogenated silicone oil = 1: (0.0005-0.0015), and control the temperature of the reactor at 70-75°C; use a sodium silicate solution with a concentration of 1.20-1.30 mol / L and a modulus of 3.4-3.5 as alkali liquid, and a sulfuric acid solution with a mass fraction of 98% as acid liquid;
[0016] S2, first step reaction: 9-10m 3 / h flow rate to add alkali solution, at the same time at 0.75-0.80m 3 / h flow rate to add acid solution, react for 25-40min, control the reaction pH at 8.5-9.0, stirring frequency 40-45Hz;
[0017] S3, second step reaction: adjust the alkali solution flow rate to 6-7m 3 / h, the acid flow rate is adjusted to 0.55-0.60m 3 / h, reaction time 30-55min, pH value of reaction controlled at 8.5-9.0, stirring frequency 50-55Hz;
[0018] S4, the third step reaction: 9-10m 3 / h flow rate to add alkali solution, at the same time at 0.75-0.80m 3 / h flow rate to add acid solution, react for 55-70min, control the reaction pH at 8.5-9.0, stirring frequency 40-45Hz;
[0019] S5. After the parallel flow reaction is completed, add acid solution to the reactor, adjust the pH value of the suspension to 7.0-7.5, and stir for 0.5-1 hour;
[0020] S6. Continue to add acid solution to the reactor, adjust the pH value of the suspension to 3.5-4.0, and age for 0.5-1 hour;
[0021] S7. The suspension treated in step S6 is washed, solid-liquid separated, pulped, and spray-dried to obtain silicon dioxide powder, thereby obtaining a qualified precipitated silica product for new energy vehicle tires.
[0022] The above-mentioned method for preparing precipitated silica for new energy vehicle tires has the following technical characteristics and beneficial effects:
[0023] 1. Step-by-step reaction to control particle size and structure: In the preparation process of white carbon black, the step-by-step reaction plays a key role in the formation and growth of crystal nuclei; in the first step of the reaction, the operation is carried out with a specific alkali and acid flow rate and reaction pH value, which is conducive to the initial formation of white carbon black crystal nuclei; the second step of the reaction controls the growth process of the crystal nuclei by adjusting the flow rate and reaction time, so that its particle size distribution is more conducive to dispersion in rubber; the third step of the reaction plays a role in stabilizing and improving the structure of white carbon black. Such a step-by-step reaction can accurately adjust the generation rate and particle size distribution of white carbon black, thereby effectively improving its dispersibility in rubber.
[0024] 2. The role of emulsified hydrogenated silicone oil: Hydrogenated silicone oil contains hydrogen-silicon structure. Si-H bond is easy to break under alkaline conditions. The hydrogen functional group can react with the surface of silica to reduce its surface energy, thereby improving the surface properties of silica. This helps to reduce the interaction force between silica particles, reduce the occurrence of agglomeration, significantly improve its dispersibility in rubber, and enable silica to play a more full reinforcing role.
[0025] 3. Effect of specific superacid and aging steps: After the co-current reaction is completed, the pH of the suspension is adjusted to 7.0-7.5 and stirred for 0.5-1 hour. Under weak alkaline conditions, the surface of the silica particles carries a negative charge, which helps to reduce the electrostatic interaction between the particles and thus reduce the tendency to agglomerate. Subsequently, the pH is adjusted to 3.5-4.0 and aged for 0.5-1 hour to further optimize the structure of silica, so that it can better combine and disperse with the rubber molecules, thereby achieving the best dispersion effect and significantly improving the performance of the tire.
[0026] 4. Reaction process setting: The present invention has simple operating steps, clear process parameters, and is easy to control and operate; the simplicity and controllability of the process are conducive to improving the stability and consistency of the product, reducing the uncertainty in the production process, reducing production costs, and improving production efficiency, and is suitable for large-scale production.
[0027] The present invention adds emulsified hydrogenated silicone oil in the reaction stage, and controls the reaction precisely in steps, so that the reaction process is more stable and controllable. After the acid-base co-current reaction is completed, a specific superacid and aging treatment process is used. The synergistic effect of each step makes the present invention not only simple and easy to implement, but also has a high yield. The prepared white carbon black can significantly improve the dispersibility of precipitated white carbon black in rubber. The highly dispersible white carbon black can meet the strict requirements of new energy vehicle tires for low rolling resistance and high grip, thereby effectively improving the performance of the tires and ensuring the safe and efficient operation of new energy vehicles. DETAILED DESCRIPTION
[0028] The preparation method of precipitated silica for new energy vehicle tires of the present invention is further described in detail below in conjunction with a specific embodiment. The specific steps are as follows:
[0029] Example 1
[0030] S1, add 60m 3 Tap water and 50kg of emulsified hydrogenated silicone oil were used as the base liquid, and the temperature of the reactor was controlled at 72°C; sodium silicate solution with a concentration of 1.20-1.30mol / L and a modulus of 3.4-3.5 was used as the alkali solution, and a sulfuric acid solution with a mass fraction of 98% was used as the acid solution;
[0031] S2, 9.5m 3 / h flow rate to add alkali solution, at the same time at 0.78m 3 Acid solution was added at a flow rate of / h, reacted for 30min, pH of the reaction was controlled at 8.8, and the stirring frequency was 45Hz;
[0032] S3, adjust the alkali solution flow rate to 6.5m 3 / h, the acid flow rate is adjusted to 0.58m 3 / h, reaction time 40min, reaction pH controlled at 8.8, stirring frequency 55Hz;
[0033] S4, adjust the alkali solution flow rate to 9.5m 3 / h, the acid flow rate is adjusted to 0.78m 3 / h, reaction time 60min, reaction pH controlled at 8.8, stirring frequency 45Hz;
[0034] S5. After the three-step acid-base co-current reaction is completed, acid solution is added to the reactor, the pH value of the suspension is adjusted to 7.2, and stirred for 0.8 hours;
[0035] S6, continue to add acid solution to the reactor, adjust the pH value of the suspension to 3.8, and age for 0.8 hours;
[0036] S7. The treated suspension is washed, solid-liquid separated, pulped, and spray-dried to obtain silicon dioxide powder, thereby obtaining qualified precipitated silica products for new energy vehicle tires.
[0037] Example 2
[0038] S1, add 60m 3 Tap water and 30kg of emulsified hydrogenated silicone oil were used as the base liquid, and the temperature of the reactor was controlled at 70.5°C; sodium silicate solution with a concentration of 1.20-1.30mol / L and a modulus of 3.4-3.5 was used as the alkali solution, and a sulfuric acid solution with a mass fraction of 98% was used as the acid solution;
[0039] S2, 9m 3 / h flow rate to add alkali solution, at the same time at 0.75m 3 Acid solution was added at a flow rate of / h, reacted for 30min, pH of the reaction was controlled at 8.5, and the stirring frequency was 45Hz;
[0040] S3, adjust the alkali solution flow rate to 6m 3 / h, the acid flow rate is adjusted to 0.55m 3 / h, reaction time 40min, reaction pH controlled at 8.5, stirring frequency 55Hz;
[0041] S4, adjust the alkali solution flow rate to 9m 3 / h, the acid flow rate is adjusted to 0.75m 3 / h, reaction time 60min, reaction pH controlled at 8.5, stirring frequency 45Hz;
[0042] S5. After the three-step acid-base co-current reaction is completed, acid solution is added to the reactor, the pH value of the suspension is adjusted to 7.0, and stirred for 0.5 hours;
[0043] S6, continue to add acid solution to the reactor, adjust the pH value of the suspension to 3.5, and age for 0.5 hours;
[0044] S7. The treated suspension is washed, solid-liquid separated, pulped, and spray-dried to obtain silicon dioxide powder, thereby obtaining qualified precipitated silica products for new energy vehicle tires.
[0045] Example 3
[0046] S1, add 60m 3 Tap water and 100kg of emulsified hydrogenated silicone oil were used as the base liquid, and the temperature of the reactor was controlled at 74°C; sodium silicate solution with a concentration of 1.20-1.30mol / L and a modulus of 3.4-3.5 was used as the alkali solution, and sulfuric acid solution with a mass fraction of 98% was used as the acid solution;
[0047] S2, 10m 3 / h flow rate to add alkali solution, at the same time at 0.8m 3 Acid solution was added at a flow rate of / h, reacted for 30min, the reaction pH was controlled at 8.5, and the stirring frequency was 43Hz;
[0048] S3, adjust the alkali solution flow rate to 7m 3 / h, the acid flow rate is adjusted to 0.6m 3 / h, reaction time 40min, reaction pH controlled at 8.5, stirring frequency 53Hz;
[0049] S4, adjust the alkali solution flow rate to 10m 3 / h, the acid flow rate is adjusted to 0.8m 3 / h, reaction time 60min, reaction pH controlled at 8.5, stirring frequency 43Hz;
[0050] S5. After the three-step acid-base co-current reaction is completed, acid solution is added to the reactor, the pH value of the suspension is adjusted to 7.5, and stirred for 1 hour;
[0051] S6, continue to add acid solution to the reactor, adjust the pH value of the suspension to 4.0, and age for 1 hour;
[0052] S7. The treated suspension is washed, solid-liquid separated, pulped, and spray-dried to obtain silicon dioxide powder, thereby obtaining qualified precipitated silica products for new energy vehicle tires.
[0053] Comparative Example 1
[0054] The difference from Example 1 is that no emulsified hydrogenated silicone oil is added in the step, and the other conditions are the same as Example 1.
[0055] Comparative Example 2
[0056] The difference from Example 1 is that after the three-step acid-base co-current reaction is completed, the step of superacidification to pH 7.2 and stirring for 0.8 hour is not performed, but the pH is directly superacidified to pH 3.8 and aged for 0.8 hour. The other conditions are the same as in Example 1.
[0057] Comparative Example 3
[0058] The difference from Example 1 is that after the three-step acid-base parallel flow reaction is completed, the acid is firstly increased to pH 7.2, stirred for 0.2 hours, and then increased to pH 3.8. The aging time is 0.2 hours. The other conditions are the same as in Example 1.
[0059] Comparative Example 4
[0060] The difference from Example 1 is that after the three-step acid-base co-current reaction is completed, the solution is firstly super-acidified to pH 6.5, stirred for 0.8 hour, then super-acidified to pH 3.8, and aged for 0.8 hour. The other conditions are the same as those in Example 1.
[0061] The test technical indicators of the white carbon black products obtained in the above embodiments and comparative examples are shown in Table 1:
[0062] Table 1 Comparison of the testing technical indicators of white carbon black products obtained from three embodiments and four comparative examples
[0063]
[0064] It can be seen from Table 1 that the silica prepared in Examples 1-3 of the present invention has good performance. Compared with the comparative example, it has obvious advantages in specific surface area, oil absorption value, dispersion, grip index, rolling resistance coefficient and tensile strength, and can meet the requirements of new energy vehicle tires for low rolling resistance and high grip.
[0065] The present invention improves the dispersibility of white carbon black in rubber through synergistic effects from multiple aspects, thereby significantly improving the performance of new energy tires, reducing rolling resistance, and improving grip, thereby ensuring the safe and efficient operation of new energy vehicles.
[0066] It should be noted that the above embodiments are not intended to limit the present invention. For those skilled in the art, they can still modify the technical solutions recorded in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing precipitated silica for new energy vehicle tires, characterized in that: It includes the following steps: S1. Preparation of acid-base co-current reaction materials: Add tap water and emulsified hydrogenated silicone oil as base liquid into the reactor, with a mass ratio of tap water: emulsified hydrogenated silicone oil = 1: (0.0005-0.0015), and control the temperature of the reactor at 70-75°C; use a sodium silicate solution with a concentration of 1.20-1.30 mol / L and a modulus of 3.4-3.5 as alkali liquid, and a sulfuric acid solution with a mass fraction of 98% as acid liquid; S2, first step reaction: 9-10m 3 / h flow rate to add alkali solution, at the same time at 0.75-0.80m 3 / h flow rate to add acid solution, react for 25-40min, control the reaction pH at 8.5-9.0, stirring frequency 40-45Hz; S3, second step reaction: adjust the alkali solution flow rate to 6-7m 3 / h, the acid flow rate is adjusted to 0.55-0.60m 3 / h, reaction time 30-55min, pH value of reaction controlled at 8.5-9.0, stirring frequency 50-55Hz; S4, the third step reaction: 9-10m 3 / h flow rate to add alkali solution, at the same time at 0.75-0.80m 3 / h flow rate to add acid solution, react for 55-70min, control the reaction pH at 8.5-9.0, stirring frequency 40-45Hz; S5. After the parallel flow reaction is completed, add acid solution to the reactor, adjust the pH value of the suspension to 7.0-7.5, and stir for 0.5-1 hour; S6. Continue to add acid solution to the reactor, adjust the pH value of the suspension to 3.5-4.0, and age for 0.5-1 hour; S7. The suspension treated in step S6 is washed, solid-liquid separated, pulped, and spray-dried to obtain silicon dioxide powder, thereby obtaining a qualified precipitated silica product for new energy vehicle tires.
Citation Information
Patent Citations
Preparation method of high-structure degree, high-specific surface area and high-dispersion white carbon black
CN110156033A
Wet-skid-resistant precipitated silicon dioxide as well as preparation method and application thereof
CN112678837A
Preparation method of precipitated silica used for high-performance tire
CN112777602A
Preparation method of high-dispersion white carbon black
CN113753905A
Preparation method of large-pore-volume precipitation-method white carbon black
CN113830773A
Cited By
Production method of white carbon black with high specific surface area and high dispersion
CN120483173A
A method for producing high specific surface area and high dispersion white carbon black