Preparation method of cuprous sulfide on carbon cloth and application of cuprous sulfide in field of friction nano-generators
The preparation of cuprous sulfide nanoparticles on carbon cloth substrates by electroplating and chemical vapor deposition methods has solved the problems of high preparation costs and complex processes in the prior art, and achieved the preparation of high-performance cuprous sulfide nanoparticles and improved friction nanometers Energy conversion performance and stability of generators.
Patent Information
- Application Number
- CN202310605816.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to efficiently prepare high-performance copper sulfide nanoparticles on flexible substrates, which limits their application in friction nanogenerators, and is highly prepared and complicated.
Using a method of combining electroplating and chemical vapor deposition, the carbon cloth is used as the substrate to grow cuprous sulfide nanoparticles through plasma treatment and chemical vapor deposition, controlling their crystal structure and morphology, and improving their electrical properties and mechanical stability.
It realizes the low-cost and efficient preparation of high-quality copper sulfide nanoparticles on carbon cloth substrates, improves the energy conversion performance and stability of friction nanogenerators, and is suitable for self-powered fields.
Smart Images

Figure CN119018927A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing three-dimensional nanoparticles by combining electroplating and chemical vapor deposition, and specifically relates to a method for preparing cuprous sulfide nanoparticles and the application of a friction nanogenerator. Background Art
[0002] In the field of triboelectric nanogenerators, triboelectric nanogenerator technology is an emerging field that uses friction motion to generate electrical energy and has broad application prospects. It uses mechanical motion at the nanoscale to convert into electrical energy, providing a sustainable energy solution for low-power electronic devices such as self-powered micro-nano systems and wearable devices. Finding efficient energy conversion materials has always been the focus of research. In traditional energy harvesting technology, due to the high energy conversion efficiency caused by friction motion at the nanoscale, triboelectric nanogenerator technology can achieve high-efficiency energy conversion and generate usable electrical energy from tiny mechanical energy input. Triboelectric nanogenerator technology does not require external energy input and can achieve self-powered power only by relying on mechanical motion or vibration in the environment, without battery replacement or charging. Compared with traditional energy harvesting technology, triboelectric nanogenerator technology has a lower environmental impact. It does not rely on limited resources such as fossil fuels, and the generated electricity is a renewable and clean energy source. In order to achieve efficient energy conversion, it is necessary to develop materials with excellent mechanical and electrical properties. These materials should have good flexibility and wear resistance, and can produce charge separation and transmission at the microscale. Triboelectric nanogenerator technology involves the conversion process between mechanical energy and electrical energy, and the design and engineering of the interface are crucial to the energy conversion efficiency. By optimizing the interface structure and contact characteristics, the energy conversion efficiency can be improved and the energy loss can be reduced. At present, a potential material is cuprous sulfide (Cu2S), which has good electrical properties and mechanical stability. However, to apply cuprous sulfide in triboelectric nanogenerators, the key issue is how to prepare cuprous sulfide nanomaterials with high performance. Carbon cloth has the characteristics of high conductivity, flexibility and tearability, can provide good mechanical support and electron transmission path, and has good chemical stability. This makes carbon cloth an ideal substrate material for preparing cuprous sulfide nanoparticles. However, there are still some challenges for the method of preparing cuprous sulfide on carbon cloth. For example, how to achieve highly uniform and continuous deposition of cuprous sulfide nanoparticles, and how to control the crystal structure and morphology of cuprous sulfide to improve its electrical properties and mechanical stability still need further research and solution. Therefore, it is necessary to propose an effective preparation method that can prepare high-quality cuprous sulfide nanoparticles on carbon cloth and control their morphology and crystal structure to meet the demand for high-performance energy conversion materials in the field of triboelectric nanogenerators. In traditional preparation methods, cuprous sulfide nanoparticles are usually prepared on hard substrates, which limits their application in flexible and bendable devices. In order to solve this problem, in recent years, researchers have begun to focus on the preparation of cuprous sulfide nanomaterials on flexible substrates, among which carbon cloth has been widely studied and applied as an ideal flexible substrate material. Therefore, it is necessary to invent a method for preparing cuprous sulfide nanoparticles with low preparation cost, high power generation performance, wide application range, and the ability to obtain high performance in the field of friction nanopower generation. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing cuprous sulfide on a carbon cloth substrate in view of the problems of high preparation cost and complicated preparation process of existing cuprous sulfide power generation materials. The method adopts a combination of electroplating and chemical vapor deposition, uses sulfur powder as a precursor, selects carbon cloth with copper particles deposited as a substrate, and uses a tubular furnace to grow cuprous sulfide nanomaterials. The method is simple and reliable, low in cost, and has good repeatability, and can synthesize cuprous sulfide nanoparticles in large quantities.
[0004] Another object of the present invention is to provide cuprous sulfide nanoparticles obtained by the above method, and to change the adhesion of the copper particles by controlling the plasma power to achieve application in the field of friction nanogenerators.
[0005] The purpose of the present invention is achieved through the following technical solutions.
[0006] A method for preparing cuprous sulfide nanoparticles and application of a friction nanogenerator comprises the following steps:
[0007] Step 1, the carbon cloth is cleaned by ultrasonic cleaning and then dried, and then plasma treated to increase its surface defects and change its surface hydrophilicity. The power of the carbon cloth plasma is set to 10W, 35W, and 60W;
[0008] Step 2, electroplating copper particles on the carbon cloth substrate through an electrolytic cell, ensuring that the copper particles can completely cover the surface of the carbon cloth and have good adhesion, and drying it at room temperature. The voltage used in the electroplating process is 4V, and the electroplating time is 5 minutes to ensure a large amount of copper particles.
[0009] Step 3, the carbon cloth substrate with copper particles deposited thereon is grown by chemical vapor deposition, the copper particles on the surface of the carbon cloth are sulfided, and cuprous sulfide nanoparticles with high crystallization quality are synthesized. The distance between the carbon cloth substrate and the sulfur powder is 10 cm, the growth time is 30 minutes, and the set heating temperature of the carbon cloth substrate is preferably 600°C.
[0010] In step 3, the flow rates of argon and hydrogen are 40 standard cubic centimeters per minute (sccm) and 10 standard cubic centimeters per minute (sccm), respectively, and the carrier gas volume ratio of argon and hydrogen is 4:1.
[0011] In step 3, the heating rates of the sulfur powder and the substrate are both 10° C. / min.
[0012] The present invention also provides the use of cuprous sulfide nanoparticles obtained by the method in a friction nanogenerator.
[0013] Advantages and beneficial effects of the present invention:
[0014] The present invention prepares cuprous sulfide nanoparticles by combining electroplating with chemical vapor deposition under the condition of using carbon cloth as a substrate. The method has the advantages of being simple, low cost, good controllability, etc. The prepared cuprous sulfide nanoparticles have a high loading amount and many active sites. The hydrophilicity of the carbon cloth can be regulated by the power of the plasma treatment process, and the loading amount of the copper particles can be further regulated. The method has good performance in a friction nanogenerator and is expected to be applied in the field of self-powered electricity. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a scanning electron microscope image of cuprous sulfide prepared in Example 1 of the present invention.
[0016] Figure 2 This is a scanning electron microscope image of cuprous sulfide prepared in Example 2 of the present invention.
[0017] Figure 3 This is the corresponding high-resolution transmission electron microscope image of cuprous sulfide prepared in Example 2 of the present invention.
[0018] Figure 4 This is a scanning electron microscope image of cuprous sulfide prepared in Example 3 of the present invention.
[0019] Figure 5 This is a schematic diagram of the structure of the friction nanogenerator prepared in Example 4 of the present invention.
[0020] Figure 6 This is the output current of the friction nanogenerator prepared in Example 4 of the present invention.
[0021] Figure 7 This is the output current of the friction nanogenerator prepared in Example 5 of the present invention.
[0022] Figure 8 This is the output current of the friction nanogenerator prepared in Example 6 of the present invention. DETAILED DESCRIPTION
[0023] The present invention uses sulfur powder as a precursor, adopts a combination of electroplating and chemical vapor deposition, and uses carbon cloth as a substrate to prepare cuprous sulfide nanoparticles with extremely high loading. The preferred embodiment of the present invention is further described below in conjunction with the accompanying drawings and specific examples.
[0024] The furnace body is a SK-G04123K single temperature zone open vacuum / atmosphere tube furnace produced by Tianjin Zhonghuan Experimental Electric Furnace Co., Ltd. (the diameter of the quartz tube in the furnace body is 40 mm). The precursor is 99.999% pure sulfur powder produced by Alfa Aesar. The carbon cloth substrate used in Examples 1-3 is laboratory carbon cloth.
[0025] Example 1
[0026] A method for preparing cuprous sulfide nanoparticles and application of a friction nanogenerator comprises the following steps:
[0027] Step 1, the carbon cloth is cleaned by ultrasonic cleaning and then dried, and then plasma treated to increase its surface defects and change its surface hydrophilicity. The power of the carbon cloth plasma is set to 10W;
[0028] Step 2, electroplating copper particles on the carbon cloth substrate through an electrolytic cell, ensuring that the copper particles can completely cover the surface of the carbon cloth and have good adhesion, and drying it at room temperature. The voltage used in the electroplating process is 4V, and the electroplating time is 5 minutes to ensure a large amount of copper particles.
[0029] Step 3, the carbon cloth substrate with copper particles deposited thereon is grown by chemical vapor deposition, the copper particles on the surface of the carbon cloth are sulfided, and cuprous sulfide nanoparticles with high crystallization quality are synthesized. The distance between the carbon cloth substrate and the sulfur powder is 10 cm, the growth time is 30 minutes, and the set heating temperature of the carbon cloth substrate is preferably 600°C.
[0030] In step 3, the flow rates of argon and hydrogen are 40 standard cubic centimeters per minute (sccm) and 10 standard cubic centimeters per minute (sccm), respectively, and the carrier gas volume ratio of argon and hydrogen is 4:1.
[0031] In step 3, the heating rates of the sulfur powder and the substrate are both 10° C. / min.
[0032] The scanning electron microscope image of the sample obtained in Example 1 of the present invention (such as Figure 1 ), which clearly shows that the cuprous sulfide nanoparticles loading on the carbon cloth surface is low and the nanofibers of the carbon cloth are exposed.
[0033] Example 2
[0034] A method for preparing cuprous sulfide nanoparticles and application of a friction nanogenerator comprises the following steps:
[0035] Step 1, the carbon cloth is cleaned by ultrasonic cleaning and then dried, and then plasma treated to increase its surface defects and change its surface hydrophilicity. The power of the carbon cloth plasma is set to 35W;
[0036] Step 2, electroplating copper particles on the carbon cloth substrate through an electrolytic cell, ensuring that the copper particles can completely cover the surface of the carbon cloth and have good adhesion, and drying it at room temperature. The voltage used in the electroplating process is 4V, and the electroplating time is 5 minutes to ensure a large amount of copper particles.
[0037] Step 3, the carbon cloth substrate with copper particles deposited thereon is grown by chemical vapor deposition, the copper particles on the surface of the carbon cloth are sulfided, and cuprous sulfide nanoparticles with high crystallization quality are synthesized. The distance between the carbon cloth substrate and the sulfur powder is 10 cm, the growth time is 30 minutes, and the set heating temperature of the carbon cloth substrate is preferably 600°C.
[0038] In step 3, the flow rates of argon and hydrogen are 40 standard cubic centimeters per minute (sccm) and 10 standard cubic centimeters per minute (sccm), respectively, and the carrier gas volume ratio of argon and hydrogen is 4:1.
[0039] In step 3, the heating rates of the sulfur powder and the substrate are both 10° C. / min.
[0040] The scanning electron microscope image of the sample obtained in Example 2 of the present invention (such as Figure 2 The cuprous sulfide nanoparticles on the surface show a high coverage rate. Its EDS characterization and high-resolution transmission electron microscopy image ( Figure 3 The lattice spacing of the copper sulfide sample is 0.197 nm, which is consistent with the lattice information of cuprous sulfide. This shows that the lattice quality of cuprous sulfide prepared by combining electroplating and chemical vapor deposition is good.
[0041] Example 3
[0042] The difference between this embodiment and embodiment 1 is that the plasma power in step 3 is set to 60 W, and the rest is the same as embodiment 1.
[0043] The scanning electron microscope image of the sample obtained in Example 3 of the present invention (such as Figure 4 As shown), the material coverage of the surface is higher than that of Example 2.
[0044] Example 4
[0045] The cuprous sulfide nanoparticles prepared in Example 1 were subjected to triboelectric nanogenerator tests. All triboelectric nanogenerator tests were performed on a 6514 programmable electrometer system. 2 Cuprous sulfide nanoparticles grown on a carbon cloth substrate serve as positive and negative electrodes, and PET serves as a central friction layer to form a sandwich structure. Figure 5 The schematic diagram of the sandwich structure is shown. We characterized its power generation performance through an electrometer and found that when the plasma power is 10W, the output voltage of the friction nanogenerator is low, 30V, and the output current is also low, such as Figure 6 As shown, this means that the performance of the friction nanogenerator in the power supply field is poor.
[0046] Example 5
[0047] The cuprous sulfide nanoparticles prepared in Example 2 were subjected to triboelectric nanogenerator tests. All triboelectric nanogenerator tests were performed on a 6514 programmable electrometer system. 2 The cuprous sulfide nanoparticles grown on the carbon cloth substrate serve as the positive and negative electrodes, and PET serves as the central friction layer to form a sandwich structure. We characterized its power generation performance using an electrometer and found that when the plasma power was 35W, the output voltage of the friction nanogenerator increased to 60V, and the output current also increased, such as Figure 7 As shown, this means that the performance of the friction nanogenerator in the power supply field has been improved.
[0048] Example 6
[0049] The cuprous sulfide nanoparticles prepared in Example 3 were subjected to triboelectric nanogenerator tests. All triboelectric nanogenerator tests were performed on a 6514 programmable electrometer system. 2 The cuprous sulfide nanoparticles grown on the carbon cloth substrate serve as the positive and negative electrodes, and PET serves as the central friction layer to form a sandwich structure. We characterized its power generation performance through an electrometer and found that when the plasma power is 60W, the output voltage of the friction nanogenerator is significantly increased to 180V. Figure 8 As shown, the output current is also relatively high, which means that the friction nanogenerator has good performance in the field of power supply and has industrial application prospects.
[0050] The above experimental results of friction nano power generation performance show that the cuprous sulfide nanoparticles prepared on the carbon cloth have extremely high power generation activity, can work continuously for a long time and have good stability. From the perspective of industrial application, the carbon cloth and the copper content are high, the cost is low, and it has great application prospects.
Claims
1. A method for preparing cuprous sulfide on carbon cloth and its application in the field of triboelectric nanogenerators, characterized in that: The copper particles deposited on the carbon cloth substrate are sulfided into cuprous sulfide by using an electrodeposition method and a chemical vapor deposition method; The method comprises the following steps: Step 1, subjecting the carbon cloth to plasma treatment to increase surface defects and change the hydrophilicity of its surface; Step 2, electroplating copper particles on the carbon cloth substrate through an electrolytic cell to ensure that the copper particles can completely cover the surface of the carbon cloth and have good adhesion, and drying it at room temperature; Step 3, growing the carbon cloth substrate with copper particles deposited thereon by chemical vapor deposition, sulfiding the copper particles on the surface of the carbon cloth, and synthesizing cuprous sulfide nanoparticles with high crystal quality.
2. The method for preparing cuprous sulfide according to claim 1, characterized in that: In step 1, the power of the carbon cloth plasma is set to 35W.
3. The method for preparing cuprous sulfide according to claim 1, characterized in that: In step 2, the voltage used in the electroplating process is 4V and the electroplating time is 5 minutes to ensure the large amount of particles attached.
4. The method for preparing cuprous sulfide according to claim 1, characterized in that: In step 3, the distance between the carbon cloth substrate and the sulfur powder is 10 cm, and the growth time is 30 minutes.
5. The method for preparing cuprous sulfide according to claim 1, characterized in that: In step 3, the heating rate of the sulfur powder is 10°C / min, and the set heating temperature of the carbon cloth substrate is preferably 600°C.
6. Use of cuprous sulfide prepared by the method according to any one of claims 1 to 5 in a friction nanogenerator.