Colored drawing glass for photovoltaic power generation and preparation method thereof
By using metal complexes with particle size less than 1μm on the photovoltaic power generation plate for digital printing and tempering, orderly agglomerations are formed, which solves the problem that photovoltaic power generation plates are difficult to achieve high-precision decoration on the exterior walls of the building and improves the Power generation efficiency and aesthetics of the product.
Patent Information
- Application Number
- CN202411247981.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-06
AI Technical Summary
It is difficult to achieve high-precision and exquisite pattern decoration on the exterior walls of existing photovoltaic power panels. At the same time, conventional high-temperature colored glaze ink reduces the light transmittance of the protective glass and affects the power generation efficiency.
Use metal complexes with particle size less than 1μm as the component of high-temperature colored glaze ink, and digitally print them on tempered glass, and orderly agglomerates of 5μm or more are formed during heating and air cooling to achieve high-precision pattern drawing and optimization Light utilization efficiency.
It realizes high-precision pattern drawing on photovoltaic power generation boards, improves the ornamentality of the product and the efficiency of photovoltaic power generation, and ensures long-term beauty and service life.
Smart Images

Figure BDA0005031400930000061 
Figure BDA0005031400930000071 
Figure BDA0005031400930000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of high-temperature colored glaze ink for glass painting, and in particular to a colored glass for photovoltaic power generation and a preparation method thereof. Background Art
[0002] At present, under the premise of energy crisis, energy conservation and environmental protection have gradually attracted people's attention, and photovoltaic power generation is one of the key projects. Photovoltaic power generation refers to a technology that uses the photovoltaic effect of the semiconductor interface to directly convert light energy into electrical energy. Photovoltaic panels are an important component of it. Photovoltaic panels include electromagnetic sheets, protective films and protective glass. The function of the electromagnetic sheet is to absorb light energy and convert it into electrical energy. Because the electromagnetic sheet is relatively brittle, two protective films are installed on both sides of the electromagnetic sheet, and then protective glass is installed on the side of the two protective films away from the electromagnetic sheet, thereby forming a photovoltaic panel. In this way, photovoltaic panels can exist alone or be installed on the exterior walls and roofs of buildings, turning these areas into power generation areas to form green buildings.
[0003] In the prior art, people have new requirements for these photovoltaic panels installed on the exterior walls of buildings. They hope to have high-precision exquisite patterns on them, which can play a decorative role while generating electricity. However, conventional light-transmitting pigments, such as the HighChroma OIVP series produced by Xiamen Handun Optical Technology Co., Ltd., have a particle size range of 10-24μm; the pearlescent powder produced by Dongguan Chengshi Chemical Co., Ltd. has a particle size range of 5-60μm. These pigments cannot be digitally printed because the maximum output hole diameter of digital printing is 1μm. In addition, the pigments in the conventional high-temperature glaze inks used for digital printing are all metal oxides. Such high-temperature glaze inks are digitally printed on protective glass, which can easily reduce the light transmittance of the protective glass and affect the power generation efficiency of photovoltaic panels. Summary of the invention
[0004] In order to solve the problem that the existing optical pigments cannot be digitally printed, it is difficult for photovoltaic panels decorated on the exterior walls of buildings to meet people's needs for both normal power generation and high-precision exquisite patterns. The present application provides a method for preparing stained glass for photovoltaic power generation, which uses metal complexes to digitally print high-precision patterns, and then tempers the metal complexes to oxidize and generate aggregates of 5μm and above. These aggregates can generate structural colors while allowing light to reach the electromagnetic sheet behind the stained glass for optical power generation.
[0005] In a first aspect, the present application provides a method for preparing stained glass for photovoltaic power generation, which adopts the following technical solution: A method for preparing stained glass for photovoltaic power generation comprises the following steps: Cutting and edge grinding: Cut the tempered glass original sheet into tempered glass substrates, and perform edge grinding on the tempered glass substrates to obtain the glass to be painted; Printing and drying: After cleaning the glass to be painted, digitally print it with high-temperature colored glaze ink, and then dry it to obtain the printed glass; Tempering: The printed glass is heated and air-cooled to obtain painted glass for photovoltaic power generation; The high temperature colored glaze ink includes a metal complex.
[0006] By adopting the above technical solution, using metal complexes with a particle size of less than 1μm as high-temperature colored glaze ink components, combined with digital printing technology, it is possible to achieve extremely high-precision pattern drawing on the surface of tempered glass. This level of precision not only meets the needs of visual aesthetics, but also provides more creative space for the design of photovoltaic panels, making the product more personalized and artistic.
[0007] During the heating and air cooling process, the metal complex decomposes into metal oxides and forms ordered agglomerates with a particle size of 5μm or more. These agglomerates can produce rich and natural colors through complex optical effects such as light scattering, reflection or interference, which not only improves the ornamental value of the product, but also cleverly utilizes the physical properties of light and optimizes the efficiency of light utilization.
[0008] First, these agglomerates can generate structural colors while allowing light to reach the electromagnetic sheet behind the stained glass for optical power generation. In addition, when the metal complex forms agglomerates, some gaps are left between the agglomerates, further increasing the transmittance of light, thereby ensuring that the efficiency of photovoltaic power generation is not affected.
[0009] The tempered glass substrate has extremely high strength and weather resistance, and can withstand harsh outdoor environments. The metal oxide as the pigment layer also has good stability and durability, and is not easy to fade or fall off, ensuring the long-term beauty and service life of the stained glass.
[0010] The stained glass not only has the function of photovoltaic power generation, but also has the effect of artistic decoration. It can transform the exterior walls and roofs of buildings into power generation areas, while increasing the beauty and cultural connotation of the buildings. This versatility makes the product have broad application prospects in green buildings, smart homes and other fields.
[0011] Preferably, the metal complex comprises at least one of hexaaminecobalt, ferric thiocyanate, magnesium citrate, copper acetate peptide and vanadyl acetylacetonate.
[0012] By adopting the above technical scheme, complexes such as hexaamine cobalt, ferric thiocyanate, magnesium citrate, copper acetate peptide and acetylacetonato vanadyl can form sufficiently small particles in aqueous solution or appropriate solvents. These particles are less than 1μm, allowing them to be accurately deposited on the surface of tempered glass through digital printing technology. This high-precision deposition capability is the key to achieving fine patterns.
[0013] These complexes have the property of decomposing at a certain temperature. In the preparation process of stained glass, these complexes will decompose into corresponding metal oxides (such as cobalt oxide and iron oxide) by heating. This decomposition process is controllable, and the decomposition products can form orderly arranged agglomerates on the surface of the glass.
[0014] Preferably, the mass fraction of the hexaamine cobalt in the high-temperature glaze ink is 10-25wt%.
[0015] By adopting the above technical solution, the viscosity of the high temperature colored glaze ink has a direct impact on its fluidity, printing accuracy and pattern clarity. A high content of hexaamine cobalt will increase the viscosity of the high temperature colored glaze ink, resulting in a decrease in fluidity, which may cause problems such as print head clogging or uneven printing. A low content may make the pattern unclear and the overall pattern appear too light.
[0016] Preferably, the mass fraction of the ferric thiocyanate in the high-temperature glaze ink is 15-22wt%.
[0017] By adopting the above technical solution, ferric thiocyanate needs to maintain a certain stability in the high-temperature glaze ink to ensure that the high-temperature glaze ink does not undergo obvious chemical changes during storage and use. If the content of ferric thiocyanate is too low, the stability of the high-temperature glaze ink may decrease, affecting the quality and performance of the high-temperature glaze ink. The viscosity of the high-temperature glaze ink has a direct impact on the printing effect. An appropriate amount of ferric thiocyanate can help adjust the viscosity of the high-temperature glaze ink so that it has good fluidity, thereby ensuring the smooth progress of the printing process. Too high or too low a content may destroy the viscosity balance of the high-temperature glaze ink, resulting in a decrease in printing quality.
[0018] Preferably, in the tempering step, the heating temperature is 600-650°C.
[0019] By adopting the above technical solution, when the heating temperature exceeds a certain limit, the oxidation rate of the metal complex will rapidly accelerate. This will cause the oxidation reaction to proceed in large quantities in a short period of time, and the generated oxide particles may rapidly increase and aggregate together, which will affect the uniformity and aesthetics of the stained glass surface. The rapid oxidation of the metal complex at high temperature may cause the color to deviate from the expected color, and this change may be difficult to control. At the same time, due to the excessively fast oxidation rate, the generated oxide may not be stable enough and may easily change during subsequent processing or use.
[0020] When the heating temperature is too low, the oxidation rate of the metal complex will be significantly reduced. This means that the generation rate of oxide particles will be slower and may not be evenly distributed on the surface of the stained glass. Too low a heating temperature may also lead to insufficient oxidation reaction, which may also affect the color stability and durability of the stained glass.
[0021] Preferably, in the tempering step, the air cooling rate is 4-8°C / min.
[0022] By adopting the above technical solution, although a faster cooling rate can shorten the cooling time, it may also cause the oxidation reaction of the metal complex to be quickly interrupted before it is completely carried out on the glass surface, which may affect the adhesion and stability of the particles. Too fast a cooling rate may cause the temperature gradient on the glass surface to be too large, so that the oxidized particles are affected by uneven stress during distribution and fixation. This uneven stress distribution may promote the agglomeration of particles or cause uneven distribution of particles, affecting the flatness and aesthetics of the glass surface.
[0023] When the air cooling speed is too slow, the glass is kept at a higher temperature for a longer time, which may cause the oxidation reaction of the metal complex to proceed excessively. If the cooling speed is too slow and improperly controlled, the oxidized particles that have been formed may lose their adhesion and fall off due to long-term high temperature. These fallen particles may contaminate the production line or affect subsequent processing.
[0024] Preferably, in the tempering step, oxygen is also added during heating.
[0025] By adopting the above technical solution, oxygen, as an oxidant, can accept electrons and reduce its own valence, thereby initiating or accelerating the oxidation reaction of the metal complex. In the oxidation reaction, the metal complex loses electrons and increases its valence to form the corresponding oxide. Generally, the oxidation reaction of the metal complex requires a higher temperature to be effective. However, when oxygen is added, the presence of oxygen promotes the transfer of electrons and the increase in the reaction rate, so that the oxidation reaction can start at a lower temperature (such as 300-400°C).
[0026] The addition of oxygen allows the oxidation reaction to proceed smoothly at a lower temperature, avoiding the violent reaction and uncontrollable situation that may occur at high temperature. This helps to reduce the problems of stress concentration and crack generation caused by overly violent reaction. The presence of oxygen promotes the transfer of electrons and the increase of reaction rate, thereby improving the oxidation efficiency. This means that more and more stable oxides can be generated in the same amount of time, which is conducive to the subsequent tempering process.
[0027] Preferably, in the tempering step, the volume fraction of oxygen in the heating reaction container is 5-10%.
[0028] By adopting the above technical solution, when the oxygen volume fraction is too large, the oxygen concentration in the reaction vessel increases significantly, thereby promoting the contact and reaction between the metal complex and oxygen. However, too high an oxygen concentration will cause the oxidation reaction rate to be too fast, making the oxidation process difficult to control. This may lead to the formation of an oxide film that is not uniform or dense enough, and may even cause problems such as local overheating and stress concentration. Too low an oxygen concentration cannot fully exert the promoting effect of the oxidant, resulting in unsatisfactory efficiency and effect of the oxidation reaction.
[0029] In a second aspect, the present application provides a stained glass for photovoltaic power generation, which adopts the following technical solution: A stained glass for photovoltaic power generation is prepared by the above-mentioned method for preparing stained glass for photovoltaic power generation.
[0030] By adopting the above technical solution, the advantages of the stained glass used for photovoltaic power generation over the prior art are the same as the above preparation method, which will not be repeated here.
[0031] In summary, this application has the following beneficial effects: 1. This application uses metal complexes in high-temperature colored glaze inks to enable them to spray patterns normally and smoothly, and then tempers the metal complexes to oxidize them to generate metal oxides that aggregate to form ordered aggregates with a particle size of 5 μm or more. These aggregates can generate structural colors while allowing light to reach the electromagnetic sheet behind the colored glass for optical power generation. In addition, the gaps between the aggregates further increase the transmittance of light, thereby ensuring that the efficiency of photovoltaic power generation is not affected; 2. The stained glass not only has the function of photovoltaic power generation, but also has the effect of artistic decoration. It can transform the exterior walls and roofs of buildings into power generation areas, while increasing the beauty and cultural connotation of the buildings. This versatility makes the product have broad application prospects in green buildings, smart homes and other fields. DETAILED DESCRIPTION
[0032] The raw materials in this application include the following parts: Hexaamminecobalt: a commercially available product with CAS number 10534-86-8 is used; Ferric thiocyanate: a commercially available product with CAS number 4119-52-2; Magnesium citrate: a commercially available product with CAS number 144-23-0; Copper acetate peptide: a commercially available product with CAS number 130120-57-9 is used; Vanadyl acetylacetonate: a commercially available product with CAS number 3153-26-2; Oxygen: a commercially available product with CAS number 7782-44-7 was used; The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0033] Example 1 A method for preparing high-temperature colored glaze ink for glass inkjet printing comprises the following steps: 1. Preparation of glass frit 6 mol of Zn(NO 3 ) 2 .6H 2 O, 3 mol Mg(NO 3 ) 2 , 1.5 mol LiNO 3 , 1 mol of Al(NO 3 ) 3 .9H 2 O, 0.3 mol Zr(NO 3 ) 4 .5H 2 O, add 1000g of water and heat to dissolve to obtain material (A); 4 mol of HBO 3 Dissolve in 300g hot water to obtain material (B); 1 mol of TiCl 4 Dissolve in 200g hot water to obtain material (C); weigh 1500g SiO 2 The mass fraction of silica sol is 40%, and material (D) is obtained. Material (A), (B), and (C) are sequentially added to material (D) under stirring at 200rpm to obtain a mixed slurry, and the prepared slurry is formed into microspheres in a 15000rpm spray dryer, and finally calcined at 590℃ for 1.5h in a rotary calcining furnace with an inner diameter of 89mm and a length of 1700mm (φ89×1700mm) to obtain a glass frit.
[0034] (2) Mixing preparation Weigh 200g of hexaaminecobalt and 750g of glass frit, add to 10g of dispersant, and make up to 1000g with water. At this time, the mass fraction of hexaaminecobalt in the high-temperature glaze ink is 20wt%. Then disperse it with a disperser at 2000rpm for 1h, and then grind it with a sand mill until the solid phase particles D99 are 1000nm. Filter through a 1000nm filter membrane to obtain the high-temperature glaze ink.
[0035] A method for preparing stained glass for photovoltaic power generation comprises the following steps: Cutting and edge grinding: Cut the original tempered glass into 50cm*50cm tempered glass substrates, and grind the tempered glass substrates to obtain the glass to be painted; Printing and drying: After cleaning the glass to be painted, use 500g of high-temperature colored glaze ink for color printing, with a printing thickness of 30μm, and cover the entire surface with high-temperature colored glaze ink (partial coverage is also possible in actual applications, but this application performs full coverage, just to better compare the visible light transmittance), and then dry to obtain the printed glass; Tempering: The painted glass is placed in a tempering furnace for heating and air cooling, with a heating temperature of 630°C, a heating time of 15 min, a cooling rate of 6°C / h, and a cooling time of 6 min to obtain painted glass for photovoltaic power generation.
[0036] Example 2-3 Example 2-3 Based on the preparation method of Example 1, the mass fraction of hexaamminecobalt is adjusted, and the specific adjustment is shown in Table 1.
[0037] Comparative Example 1-2 Comparative Example 1-2 Based on the preparation method of Example 1, the mass fraction of hexaamminecobalt was adjusted, and the specific adjustment is shown in Table 1.
[0038] Comparative Example 3 Comparative Example 3: Based on the preparation method of Example 1, the hexaammine cobalt is replaced with cobalt oxide, and other conditions remain unchanged.
[0039] Table 1 Mass fraction and performance test table of hexaammine cobalt of Examples 1-3 and Comparative Examples 1-3 Performance Test The stained glass for photovoltaic power generation of Examples 1-3 and Comparative Examples 1-3 was subjected to the following performance tests, and the test results are shown in Table 1: 1. Light transmittance of glass The light transmittance of the painted glass used for photovoltaic power generation is measured according to GBA2680 "Determination of visible light transmittance of architectural glass".
[0040] 2. Adhesion of high temperature glaze ink The adhesion fastness of high temperature colored glaze ink was determined according to the method of GB / T13217.7.
[0041] Referring to Table 1, by comparing Examples 1-3 and Comparative Examples 1-3, it can be seen that compared with Comparative Example 3, the visible light transmittance and adhesion fastness of Examples 1-3 are much higher than those of Comparative Example 3, indicating that the use of metal complexes instead of metal oxides in high-temperature glaze inks for digital printing on glass, and then tempering, can effectively oxidize and aggregate the metal complexes, so that the painted glass does not affect power generation and can prepare extremely high-precision patterns. However, when oxides are directly digitally printed on tempered glass, the aggregation effect is not good.
[0042] As the mass fraction of cobalt hexaamine increases, the visible light transmittance and adhesion strength both show a trend of first increasing and then decreasing. This may be because as the mass fraction of cobalt hexaamine increases, cobalt hexaamine is continuously oxidized and the oxides are continuously agglomerated. As the number of agglomerated particles increases, the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink are improved. When the mass fraction of cobalt hexaamine exceeds a certain range, the viscosity of the high-temperature glaze ink will increase, resulting in a decrease in fluidity, which may cause problems such as print head clogging or uneven printing, thereby affecting the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink.
[0043] Embodiment 4-6 Example 4 Based on the preparation method of Example 1, the hexaaminecobalt is replaced with ferric thiocyanate, and other conditions remain unchanged.
[0044] Example 5-6 Based on the preparation method of Example 4, the mass fraction of ferric thiocyanate was adjusted, and the specific adjustment is shown in Table 2.
[0045] Comparative Examples 4-5 Comparative Example 4-5 Based on the preparation method of Example 4, the mass fraction of ferric thiocyanate was adjusted, and the specific adjustment is shown in Table 2.
[0046] The stained glass for photovoltaic power generation of Examples 4-6 and Comparative Examples 4-5 were subjected to the above performance tests, and the test results are shown in Table 2.
[0047] Table 2 Mass fraction and performance test table of ferric thiocyanate of Example 1, Examples 4-6 and Comparative Examples 4-5 project Example 1 Example 4 Example 5 Example 6 Comparative Example 4 Comparative Example 5 Ferric thiocyanate / wt% / 20 15 22 13 25 Visible light transmittance / % 92.5 92.1 82.3 84.7 77.6 79.8 Adhesion fastness / % 94.7 94.5 89.4 93.7 86.5 91.8 Referring to Table 2, by comparing Example 1, Examples 4-6 and Comparative Examples 4-5, it can be seen that ferric thiocyanate can still be used in the present application. In comparison, the effect of hexaaminecobalt is slightly higher than that of ferric thiocyanate, and Example 1 is preferred.
[0048] As the mass fraction of ferric thiocyanate continues to increase, the visible light transmittance and adhesion fastness both show a trend of first increasing and then decreasing. This may be because as the mass fraction of ferric thiocyanate continues to increase, ferric thiocyanate continues to oxidize, and the oxides continue to agglomerate. As the agglomerated particles increase, the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink are improved; when the mass fraction of ferric thiocyanate exceeds a certain range, the viscosity of the high-temperature glaze ink will increase, resulting in a decrease in fluidity, which may cause problems such as print head clogging or uneven printing, thereby affecting the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink.
[0049] Embodiment 7-8 In Examples 7-8, based on the preparation method of Example 1, the heating temperature was adjusted. The specific adjustments are shown in Table 3.
[0050] Comparative Examples 6-7 In Comparative Example 6-7, based on the preparation method of Example 1, the heating temperature was adjusted. The specific adjustments are shown in Table 3.
[0051] The stained glass for photovoltaic power generation of Examples 7-8 and Comparative Examples 6-7 were subjected to the above performance tests, and the test results are shown in Table 3.
[0052] Table 3 Heating temperature and performance test table of Example 1, Examples 7-8 and Comparative Examples 6-7 Referring to Table 3, by comparing Example 1, Examples 7-8 and Comparative Examples 6-7, it can be seen that as the heating temperature continues to increase, the visible light transmittance and the adhesion fastness show a trend of first increasing and then decreasing. This may be because as the heating temperature continues to increase, the generated oxide particles gradually gather together, thereby increasing the light transmittance of the painted glass and the adhesion of the high-temperature glaze ink; when the heating temperature exceeds a certain range, the oxidation reaction proceeds in large quantities in a short period of time. Due to the excessively fast oxidation rate, the generated oxide may not be stable enough, thereby reducing the light transmittance of the painted glass and the adhesion of the high-temperature glaze ink.
[0053] Examples 9-10 In Examples 9-10, based on the preparation method of Example 1, the cooling rate is adjusted, and the specific adjustments are shown in Table 4.
[0054] Comparative Examples 8-9 In Comparative Examples 8-9, based on the preparation method of Example 1, the cooling rate was adjusted, and the specific adjustments are shown in Table 4.
[0055] The stained glass for photovoltaic power generation of Examples 9-10 and Comparative Examples 8-9 was subjected to the above performance tests, and the test results are shown in Table 4.
[0056] Table 4 Cooling rate and performance test table of Example 1, Examples 9-10 and Comparative Examples 8-9 project Example 1 Example 9 Example 10 Comparative Example 8 Comparative Example 9 Cooling rate / (℃ / min) 6 4 8 3 9 Visible light transmittance / % 92.5 84.0 89.7 78.9 85.5 Adhesion fastness / % 94.7 89.9 92.3 88.5 91.2 Referring to Table 4, by comparing Example 1, Examples 9-10 and Comparative Examples 8-9, it can be seen that as the cooling rate continues to increase, the visible light transmittance and the adhesion fastness both show a trend of first increasing and then decreasing. This may be because as the cooling rate continues to increase, the oxidation reaction continues to proceed in an orderly manner, and the oxides gradually agglomerate, thereby increasing the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink; when it exceeds a certain range, the oxidation reaction of the metal complex may be quickly interrupted before it is completely carried out on the glass surface, which may affect the adhesion and stability of the particles, thereby reducing the light transmittance of the stained glass and the adhesion of the high-temperature glaze ink.
[0057] Examples 11-13 Example 11 is based on the preparation method of Example 1, and oxygen is also introduced during heating, the volume fraction of oxygen is 8% of the tempering furnace, the heating temperature is 610° C., and other conditions remain unchanged.
[0058] In Examples 12-13, based on the preparation method of Example 11, the volume fraction of oxygen is adjusted, and the specific adjustments are shown in Table 5.
[0059] Comparative Examples 10-11 Comparative Examples 10-11 are based on the preparation method of Example 11, except that the volume fraction of oxygen is adjusted. The specific adjustments are shown in Table 5.
[0060] The stained glass for photovoltaic power generation of Examples 11-13 and Comparative Examples 10-11 was subjected to the above performance tests, and the test results are shown in Table 5 respectively.
[0061] Table 5 Oxygen volume fraction and performance test table of Example 1, Examples 11-13 and Comparative Examples 10-11 Referring to Table 5, by comparing Example 1, Examples 11-13 and Comparative Examples 10-11, it can be seen that the introduction of oxygen during heating can more effectively improve the visible light projection ratio and the adhesion strength at a lower heating temperature. This may be because the lower heating temperature makes the oxidation reaction more gentle, while the increase in oxygen increases the overall degree of oxidation, which not only increases the progress of the oxidation reaction and improves the visible light projection ratio, but also makes the entire oxidation reaction more gentle, thereby improving the adhesion strength.
[0062] Examples 14-16 In Examples 14-16, based on the preparation method of Example 1, the type of metal complex was adjusted, and other conditions remained unchanged. The specific adjustments are shown in Table 6.
[0063] The stained glass for photovoltaic power generation of Examples 14-16 was subjected to the above performance tests, and the test results are shown in Table 6 respectively.
[0064] Table 6 Types and performance test table of metal complexes of Example 1 and Examples 14-16 project Example 1 Embodiment 14 Embodiment 15 Example 16 Metal complex type Hexaamminecobalt Magnesium Citrate Copper acetate peptide Vanadyl acetylacetonate Visible light transmittance / % 92.5 91.8 91.6 91.3 Adhesion fastness / % 94.7 94.1 93.5 93.7 Referring to Table 6, it can be seen from the comparison between Example 1 and Examples 14-16 that magnesium citrate, copper acetate peptide and vanadyl acetylacetonate can all be used in the present application.
[0065] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing stained glass for photovoltaic power generation, characterized in that: The following steps are involved: Cutting and edge grinding: Cut the tempered glass original sheet into tempered glass substrates, and perform edge grinding on the tempered glass substrates to obtain the glass to be painted; Printing and drying: After cleaning the glass to be painted, digitally print it with high-temperature colored glaze ink, and then dry it to obtain the printed glass; Tempering: The printed glass is heated and air-cooled to obtain painted glass for photovoltaic power generation; The high temperature colored glaze ink includes a metal complex.
2. The method for preparing stained glass for photovoltaic power generation according to claim 1, characterized in that: The metal complex comprises at least one of hexaaminecobalt, ferric thiocyanate, magnesium citrate, copper acetate peptide and vanadyl acetylacetonate.
3. The method for preparing stained glass for photovoltaic power generation according to claim 2, characterized in that: The mass fraction of the hexaammine cobalt in the high-temperature colored glaze ink is 10-25wt%.
4. The method for preparing stained glass for photovoltaic power generation according to claim 2, characterized in that: The mass fraction of the ferric thiocyanate in the high-temperature glaze ink is 15-22wt%.
5. The method for preparing stained glass for photovoltaic power generation according to claim 1, characterized in that: In the tempering step, the heating temperature is 600-650°C.
6. The method for preparing stained glass for photovoltaic power generation according to claim 5, characterized in that: In the tempering step, the air cooling rate is 4-8°C / min.
7. The method for preparing stained glass for photovoltaic power generation according to claim 1, characterized in that: During the tempering step, oxygen is also added during heating.
8. The method for preparing stained glass for photovoltaic power generation according to claim 7, characterized in that: In the tempering step, the volume fraction of oxygen in the heating reaction container is 5-10%.
9. A stained glass for photovoltaic power generation, characterized in that: The stained glass is prepared according to the method for preparing stained glass for photovoltaic power generation as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Conductive inks and manufacturing method thereof
CN101010388A
Enamelled tempered glass and preparation method thereof
CN108164156A
Preparation process of digital printing hollow laminated glass
CN113087416A
Colored photovoltaic backboard with high reflectivity and high barrier property
CN116574291A
Cited By
BAPV photovoltaic module, high-temperature colored glazed glass and tempering method of high-temperature colored glazed glass
CN119349874A
BAPV photovoltaic module, high temperature colored glaze glass and tempering method thereof
CN119349874B