Physical enhancement method of geopolymer sintering-free artificial aggregate based on fresh compactness and application of physical enhancement method

The physical reinforcement method of geopolymer non-sintering artificial aggregate optimized by the fresh density method solves the problems of high cost, long time, labor, cumbersome process and poor reliability in the existing technology, and achieves strength improvement, cost reduction and shortened optimization cycle, which is applicable to ultra-high performance concrete.

CN119019105AActive Publication Date: 2024-11-26SOUTH CHINA UNIV OF TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410929777.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-26
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The performance optimization of geopolymer non-sintering artificial aggregates in existing technologies suffers from high cost, long time consumption, labor-intensive and cumbersome processes, as well as poor reliability, making it difficult to widely apply in building materials.

Method used

A physical enhancement method based on fresh density was adopted. Solid precursor powder was added to a disc granulator and an alkaline activator solution was sprayed. The precursor formulation with the highest fresh density was selected. After fresh granules were obtained, they were solidified and sieved. The fresh density was tested to optimize the performance.

Benefits of technology

It significantly improves the strength of geopolymer-based non-sintering artificial aggregates, reduces raw material costs, shortens the optimization cycle, simplifies sample preparation, and improves the reliability and efficiency of optimization results, making it suitable for ultra-high performance concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019105A_ABST
    Figure CN119019105A_ABST
Patent Text Reader

Abstract

The invention discloses a physical enhancement method of geopolymer sintering-free artificial aggregate based on fresh compactness and application thereof, and the method comprises the following steps: introducing a concept of fresh compactness, and providing a performance optimization method based on the fresh compactness; according to the method, fresh compactness test is carried out on fresh particles produced by disc granulation, and a solid precursor formula corresponding to the maximum value of the fresh compactness is preferably selected for granulation and solidification, so that the high-strength geopolymer sintering-free artificial aggregate with relatively low reaction degree is prepared. According to the optimization method, the strength of the geopolymer sintering-free artificial aggregate can be remarkably improved, meanwhile, the cost is remarkably reduced, time consumption, material consumption and tedious sample preparation work needed in the optimization process can be greatly reduced, and the optimization method has the technical advantages of being efficient, rapid, time-saving, labor-saving, economical and reliable. In addition, the invention also provides an application scheme of the ultrahigh-strength geopolymer sintering-free artificial aggregate developed based on the fresh compactness in ultrahigh-performance concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial aggregate preparation, and in particular relates to a physical reinforcement method of geopolymer sinter-free artificial aggregate based on fresh density and application thereof. Background Art

[0002] Artificial aggregates are widely used in building materials, gardening materials, food hygiene materials, industrial filtration materials, radar absorbing and shielding materials, heavy metal solidification materials, oil well mining support materials and other fields due to their lightweight, porous and controllable properties. In terms of curing temperature, artificial aggregates are divided into two types: sintering and sinter-free. Among them, sinter-free artificial aggregates only need to be cured at room temperature (≤100°C) to form strength. Although this curing method is obviously greener and lower-carbon than sintering, the application of sinter-free artificial aggregates is severely restricted due to limitations such as generally lower aggregate strength, generally unstable performance levels, longer aggregate production cycles and generally higher raw material costs. Therefore, how to efficiently and reliably optimize the strength of sinter-free artificial aggregates and reduce their raw material costs has become a hot topic in many industries.

[0003] Disc granulation is the most common production method for unfired artificial aggregates. It is worth mentioning that the unfired artificial aggregates produced by the disc granulator and the traditional cast-in-place slurry materials (such as concrete, mortar, grouting materials, etc.) have fundamental differences in production process, curing method, material structure, material properties, application scenarios and performance evaluation system. For example, fresh artificial aggregates are unsaturated and non-plastic agglomerated particles, while freshly mixed concrete is an oversaturated and fluid slurry; for another example, compared with the wide application scenarios of the above-mentioned artificial aggregates, the application scenarios of concrete are usually only used as building materials. In general, unfired artificial aggregates and traditional cast-in-place slurry materials are two completely different material systems, so the design and performance optimization methods of traditional cast-in-place slurry materials are basically not applicable to unfired artificial aggregates.

[0004] In recent years, geopolymer sinter-free artificial aggregate (GCBA) has become a popular choice in the research and development of new sinter-free artificial aggregates, which is attributed to GCBA's higher strength, lower energy consumption, recycling potential in a wide range of solid wastes, and excellent heavy metal fixation capacity. The only drawback is that the existing technology still mainly relies on chemical enhancement to improve the performance of geopolymer artificial aggregates, including the use of highly active solid precursor materials (such as blast furnace slag powder, metakaolin, etc.), and the use of higher doses or higher concentrations of alkaline activator solutions, etc., all of which aim to produce more reaction products to fill the pore structure of the densified artificial aggregate and ultimately achieve strength improvement. However, this will undoubtedly cause a huge cost burden that cannot be ignored, which has largely restricted the application of geopolymer artificial aggregates. For example, the price of alkaline activator solution is about 5,000 to 7,000 yuan / ton (accounting for about 80% of the total cost), the price of blast furnace slag powder is about 600 to 800 yuan / ton, the price of kaolin is about 800 to 1,200 yuan / ton, and the price of traditional unburned artificial aggregate is only about 100 to 400 yuan / ton.

[0005] At the same time, the prior art optimization of the performance of unfired artificial aggregates is based on the hardening performance of the aggregates, such as the cylinder compressive strength after hardening, the water absorption rate after hardening, the apparent density and bulk density after hardening, etc. However, evaluating the hardening performance of aggregates often requires a long period of time (about 28 days / group) and more cumbersome sample preparation (referring to GB / T17431.2-2010, the required hardening sample volume is about 5-6 liters (bulk volume) / group). It can be seen that the existing optimization technology is a time-consuming and laborious project.

[0006] In summary, the existing technologies for optimizing the performance of geopolymer sinter-free artificial aggregates have limitations such as high cost burden, long time consumption, laboriousness, cumbersomeness, and poor reliability, which seriously restrict the development of GCBA. Summary of the invention

[0007] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0008] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0009] In order to overcome the limitations of the prior art in the above-mentioned field of geopolymer artificial aggregate technology, the present invention proposes a new reinforcement method based on physical reinforcement, which can not only achieve a significant improvement in the strength of geopolymer unfired artificial aggregate and an effective reduction in raw material costs at the same time, but also greatly shorten the time-consuming and tedious sample preparation work required for the performance optimization of geopolymer artificial aggregate, making the optimization process more efficient and time-saving and labor-saving, and can improve the reliability of the optimization results.

[0010] In order to solve the above technical problems, the present invention provides the following technical solutions: A physical reinforcement method of geopolymer sinter-free artificial aggregate based on fresh density, comprising:

[0011] The solid precursor powder of the geopolymer unburned artificial aggregate (hereinafter referred to as the precursor) is added into a disc granulator, and the alkaline activator solution is evenly sprayed on the powder in the form of mist until the fine particles are wrapped into fresh particles of the geopolymer unburned artificial aggregate of the required diameter;

[0012] Testing the fresh density of fresh particles and selecting the precursor formula with the highest fresh density;

[0013] The fresh particles prepared by using the preferred formula are solidified and sieved to obtain the sinter-free artificial aggregate based on physical reinforcement geopolymer;

[0014] Among them, fresh density is the volume V of the precursor in the fresh particle P The apparent volume V of fresh particles F The ratio is:

[0015]

[0016]

[0017] In the formula, m p and m F represent the mass of solid precursor in fresh particles and the mass of fresh particles, respectively; LSR represents liquid-solid ratio; represents the precursor material; ρ x represents the absolute density of the solid precursor component x; VR x Represents the volume ratio of the solid precursor component x to the solid precursor mixture, satisfying:

[0018]

[0019] Fresh particle apparent volume V F The fresh particles are placed in a 40-80℃ oven for constant temperature heat treatment for 5-15h, and then measured by the Archimedes drainage method after cooling;

[0020] Among them, the test of fresh density is divided into two stages: heat treatment and testing. The heat treatment stage requires 5 to 15 hours, the average testing stage requires 0.5 hours, and the total time is 6 to 16 hours; the temperature in the heat treatment stage is 40 to 80°C.

[0021] As a preferred embodiment of the method of the present invention, the precursor powder of the fresh particles is fly ash and silica ash rich in silicon and aluminum components, and solid waste brick powder with certain alkali activation activity.

[0022] As a preferred embodiment of the method of the present invention, in the precursor powder of the fresh particles, the Dv90 of waste brick powder is 65.5 μm, the Dv90 of fly ash is 39.6 μm, and the Dv90 of silica ash is 6.3 μm, and the maximum particle size of the three does not exceed 170 μm.

[0023] As a preferred embodiment of the method of the present invention, the precursor powder of the fresh particles, the powder rich in silicon and aluminum components accounts for 25 vol%, of which fly ash and silica ash account for 12.5 vol% each; the solid waste brick powder accounts for 75 vol%.

[0024] As a preferred embodiment of the method of the present invention, the alkaline activator solution is potassium water glass, with a modulus of 1.0, a mass concentration of 40%, and a liquid-to-solid ratio of 0.17.

[0025] As a preferred embodiment of the method of the present invention, the heat treatment temperature of the fresh particles used to test the fresh density is 40-80° C., and the heat treatment time is 5-15 hours.

[0026] As a preferred embodiment of the method of the present invention, the thermal curing temperature of the fresh particles is 80° C., the heat treatment time is 24 hours, and the subsequent curing time at room temperature is 28 days.

[0027] As a preferred embodiment of the method of the present invention, the maximum fresh density is 0.72, the corresponding liquid-solid ratio of fresh particles is 0.17, the cylinder compressive strength of the aggregate after solidification is above 40 MPa, and the reaction degree of the aggregate after solidification is below 8.5%.

[0028] As a preferred embodiment of the method of the present invention, the ultra-high performance concrete produced from the artificial aggregate with a cylinder compressive strength of more than 40 MPa has a 7-day compressive strength of more than 160 MPa.

[0029] The first purpose of the present invention is to overcome the limitation of the prior art of unburned artificial aggregate that the cost increases due to the increase in strength, and to provide a performance optimization method that can achieve both strength improvement and cost reduction.

[0030] The second purpose of the present invention is to overcome the limitation of the prior art of unburned artificial aggregate that a higher degree of reaction is required to synthesize higher strength artificial aggregate, and to provide a physical reinforcement method that can synthesize higher strength artificial aggregate through a mix ratio with a lower degree of reaction.

[0031] The third purpose of the present invention is to overcome the limitation of the prior art of optimizing the performance of unfired artificial aggregates, which is that the optimization results are based on specific experience and thus result in insufficient reliability of the results, and to provide a performance optimization method with clear physical meaning guidance.

[0032] The fourth object of the present invention is to overcome the limitation of the long time-consuming strength optimization cycle in the prior art of unburned artificial aggregate, and to provide a strength optimization method with an optimization cycle of only less than 16 hours.

[0033] The fifth purpose of the present invention is to overcome the limitation of large and complicated sample preparation in the prior art of performance optimization of unfired artificial aggregate, and to provide a strength optimization method that only requires about 300 ml of sample as optimization consumables.

[0034] The sixth object of the present invention is to overcome the limitation that the strength of the unsintered artificial aggregate in the prior art is generally lower than that of the natural aggregate, and to provide a high-strength geopolymer unsintered artificial aggregate developed based on the above-mentioned optimization method, whose aggregate strength is higher than that of natural pebbles.

[0035] The seventh object of the present invention is to overcome the limitation of the prior art that unfired artificial aggregates are difficult to use in ultra-high performance concrete, and to provide a high-strength geopolymer unfired artificial aggregate developed based on the above method for use in ultra-high performance concrete above 150MPa.

[0036] Beneficial effects of the present invention:

[0037] The present invention can simultaneously improve the strength and reduce the cost of geopolymer unfired artificial aggregate by innovatively introducing the fresh density method, and can also greatly reduce the time and tedious sample preparation work required for performance optimization, providing an efficient, reliable, economical, environmentally friendly and physically guided high-strength geopolymer artificial aggregate strength optimization method and its application scheme in ultra-high performance concrete, which has high technical and economic value. The details are as follows:

[0038] (1) Significant effect of improving strength: The present invention found that the strength of geopolymer unsintered artificial aggregate (GCBA) can be significantly enhanced by improving the fresh density. For example: as the fresh density increases from 0.55 to 0.72, the cylinder compressive strength of brick powder-based GCBA increases from 11.4MPa to 42.2MPa, an increase of 270%, showing a significant exponential growth. The highest cylinder compressive strength of 42.2MPa (corresponding to an average single particle strength of 20.21MP) even exceeds the strength of natural pebbles (cylinder compressive strength of about 25 to 32MPa), which is 6 times the highest strength index of light coarse artificial aggregate specified in GBT 17431.1-2010 (6.5MPa), and exceeds the strength of artificial aggregates reported in most literature. What is more worth mentioning is that GCBA with a fresh density of 0.72 and a strength of 42.2 MPa can even be used to prepare ultra-high performance concrete (UHPC) with a compressive strength of up to 162.9 MPa, which is 49.9% higher than that of UHPC using the same amount of commercial unburned artificial aggregate, and only 9.7% lower than that of UHPC using the same amount of natural coarse aggregate.

[0039] (2) It has strong robustness for strength optimization; the fresh density proposed in the present invention as an evaluation index can accurately reflect the physical stacking state of the raw materials of artificial aggregate in the initial granulation stage, so that the design method will be applicable to the strength optimization of GCBA based on various solid wastes. The present invention provides theoretical guidance with clear physical meaning for the strength optimization design of GCBA for the first time. It improves the robustness and reliability of GCBA performance optimization through physical enhancement methods, avoids the common problem that the optimization results cannot be reproduced due to the optimization parameters obtained from specific raw materials, and helps GCBA to achieve a wider range of high-value and efficient utilization of solid waste or by-products.

[0040] (3) Effectively reduce the synthesis cost, with significant economic benefits: The present invention first discovered that by improving the fresh density of GCBA, the amount of alkali activator can be effectively reduced, thereby significantly reducing the cost of GCBA raw materials. This is because the alkali activator is the largest synthesis cost of GCBA, accounting for about 80%.

[0041] (4) Shorten the optimization cycle and improve the optimization efficiency; the evaluation time period of the performance optimization method based on fresh density of the present invention is only about 16 hours, which greatly shortens the trial and error cycle compared to the evaluation time period of 28 days required by the traditional method based on hardened performance optimization. The rapid evaluation method significantly improves the production and R&D efficiency, making the development process of new materials more efficient and faster, and helps to accelerate the market application and promotion of new geopolymer artificial aggregates.

[0042] (5) Effectively reduce the consumables and tedious sample preparation work required for performance optimization, and reduce the trial and error cost; compared with the traditional optimization method based on hardening performance, which usually requires more than 5 liters of sample, the optimization method based on fresh density of the present invention only requires about 300 ml of sample, which greatly reduces the sample usage and saves the consumables required for trial and error optimization, which reduces the tedious sample preparation work and the trial and error cost, making the material performance optimization process more simple and economical, and improving the overall R&D efficiency and resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0044] Figure 1 The SEM photos of the solid precursors in the embodiments of the present invention and their particle size distribution diagrams, including (a) waste brick powder, (b) fly ash, (c) silica fume, and (d) particle size distribution.

[0045] Figure 2 It is the composition ratio and distribution diagram of the GCBA solid precursor in the embodiment of the present invention.

[0046] Figure 3 It is a fresh density contour map of fresh particles of the ternary system GCBA in the embodiment of the present invention.

[0047] Figure 4 GCBA sample diagrams with different mixing ratios in the embodiments of the present invention.

[0048] Figure 5 The relationship between the fresh density of 10 groups of GCBA in the embodiment of the present invention and the cylinder pressure strength and liquid-solid ratio.

[0049] Figure 6 It is a contour diagram of the reaction degree of the ternary system GCBA hardened particles in the embodiment of the present invention.

[0050] Figure 7 It is a contour diagram of the cylinder compressive strength of the ternary system GCBA hardened particles in the embodiment of the present invention.

[0051] Figure 8 This is an exponential relationship diagram between the fresh density and cylinder pressure strength of 10 groups of GCBA in the embodiment of the present invention.

[0052] Fig. 9 It is a comparison chart of the single particle strength of GCBA in the embodiment of the present invention and the relevant international level.

[0053] Fig.10 SEM images of GCBA hardened particles developed for different fresh densities in examples of the present invention.

[0054] Fig.11 Pore ​​structure diagram of GCBA hardened particles developed at different fresh densities in examples of the present invention.

[0055] Fig.12 This is a graph showing the compressive strength of ultra-high performance concrete produced with different coarse aggregates in an embodiment of the present invention. DETAILED DESCRIPTION

[0056] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0057] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0058] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0059] (1) Method for determining the chemical composition, ignition loss, particle size distribution, microscopic photograph and absolute density (true density) of the precursor material of the present invention:

[0060] The chemical composition can be measured by X-ray fluorescence spectrometer;

[0061] The loss on ignition can be measured by a thermogravimetric analyzer or a muffle furnace;

[0062] The particle size distribution can be measured by a laser particle size analyzer; the microscopic photograph can be measured by a SEM scanning electron microscope; the absolute density (true density) can be measured by a fully automatic true density analyzer or a Levin bottle method (such as GB / T 208-2014, etc.).

[0063] (2) Density and water absorption of hardened GCBA particles in the present invention:

[0064] The loose bulk density, dry apparent density and water absorption rate of hardened particles can be implemented in accordance with the national standard GB / T17431.2-2010.

[0065] (3) Cylinder compression strength and single particle strength of hardened GCBA particles of the present invention:

[0066] Cylinder compression strength is a commonly used indicator for evaluating the strength of artificial aggregates in China. Its test procedure can be carried out in accordance with the national standard GB / T17431.2-2010.

[0067] Single particle strength is a commonly used indicator for evaluating the strength of artificial aggregates internationally, and can be determined based on the average particle strength of 30 randomly selected GCBA particles.

[0068] (4) The method for terminating the GCBA chemical reaction of the present invention:

[0069] In order to more accurately evaluate the microscopic characteristics of GCBA (such as SEM, MIP, BSE-EDS) and the degree of reaction, the required GCBA sample should be subjected to a termination reaction treatment before testing.

[0070] (5) Degree of reaction of hardened GCBA

[0071] The test can be carried out by combining the acid etching method with the loss on ignition method, and the average value of three identical tests is taken as the test result.

[0072] (6) Method for determining the micromorphology, pore structure and phase distribution of hardened GCBA:

[0073] Microscopic morphology can be assessed by scanning electron microscopy;

[0074] The pore structure parameters can be evaluated by mercury porosimetry.

[0075] (7) Compressive strength of ultra-high performance concrete (UHPC)

[0076] The ultra-high performance concrete compressive strength test procedure can be carried out in accordance with T / CECS864-2021.

[0077] Example 1

[0078] The purpose of this example is to demonstrate the entire process of performance optimization of an ultra-high-strength GCBA based on fresh density and its application in ultra-high performance concrete.

[0079] The solid precursors used to make GCBA in this example are waste brick powder (WBP), fly ash (FA), and silica fume (SF);

[0080] (1)WBP recycling process:

[0081] First, the waste mortar attached to the surface of the waste bricks is removed manually;

[0082] Subsequently, these waste bricks are crushed into waste brick aggregates with a maximum size of 30 mm by a hammer crusher;

[0083] Finally, the waste brick aggregates were ground into WBP using a ball mill with a grinding time of 30 min and a mass ratio of grinding media to ground material of 12.5:1.

[0084] (2) FA and SF are commercially available products.

[0085] (3) According to the Chinese standard GB / T208-2014, the absolute density (true density) of WBP, FA and SF is 2.738, 2.507 and 2.241 g / cm, respectively. 3 .

[0086] Table 1 lists the chemical compositions and loss on ignition (LOI) of these solid raw materials, which were determined by X-ray fluorescence spectrometer (XRF) and thermogravimetric analyzer (TG), respectively.

[0087] Table 1

[0088]

[0089] The microscopic morphological characteristics of the solid powder were photographed using a scanning electron microscope (SEM). Figure 1 (a)-(c) are shown, and the particle size distribution is measured by laser diffraction analyzer, see Figure 1 (d).

[0090] (4) Potassium water glass (K 2 SiO 3 ) solution, modulus (SiO 2 / K 2 O molar ratio) was 1.0, the mass concentration was 40%, and the alkaline activator solution was prepared one day before its use.

[0091] (5) Mixing ratio and production process of GCBA fresh granules

[0092] In order to obtain GCBA with the highest fresh density produced by the WBP-FA-SF ternary precursor system, 10 groups of GCBA mix ratios were set, see Figure 2 .

[0093] Table 2 lists the detailed information of each combination, where the liquid-to-solid ratio represents the mass ratio of the alkaline activator solution and the solid precursor required for fresh granule production, which is determined by relevant preliminary tests comparing the granulation effect and the mass of fresh granules.

[0094] The sample names (GCBA ID.) in Table 2 represent the volume ratio of the solid precursor, for example, “90W-5F-5S” represents a GCBA sample produced from a solid precursor consisting of “90 vol% WBP, 5 vol% FA and 5 vol% SF”.

[0095] Table 2

[0096]

[0097] Production of fresh granules of GCBA using the disc granulation process:

[0098] First, 800 g of the precursor mixed powder was added into a disc granulator having a diameter of 500 mm and a disc tilt angle of 36°, and then the alkaline activator solution was evenly sprayed on the powder in the form of mist;

[0099] Initially, the granulator disc speed was set at 35-40 rpm until the powder became fine particles;

[0100] Then, the rotation speed is maintained at 15-18 rpm until the fine particles are wrapped into fresh particles of the desired diameter;

[0101] During this process, 100-200 g of precursor powder was added to the granulator every 1-2 minutes, while a certain amount of activator solution was sprayed to ensure uniform mixing until fresh granules were produced.

[0102] (6) Fresh density Tests and results:

[0103] Fresh density The test:

[0104] The volume of the precursor in the fresh particle V P The apparent volume V of fresh particles F The ratio is:

[0105]

[0106]

[0107] In the formula, m p and m F represent the mass of solid precursor in fresh particles and the mass of fresh particles, respectively; LSR represents liquid-solid ratio; represents the precursor material; ρx represents the absolute density of the solid precursor component x; VR x Represents the volume ratio of precursor component x to the solid precursor mixture, satisfying:

[0108]

[0109] Among them, the mass of fresh particles (m F );

[0110] Liquid-to-solid ratio (LSR) and volume ratio of solid precursor x (VR x ) are given in Table 2;

[0111] Fresh particle apparent volume V F The fresh particles are placed in an oven at 80°C for constant temperature heat treatment for 5 to 12 hours and then cooled down and measured using the Archimedes drainage method; the fresh density of each group of samples is the average of three identical tests, with approximately 100 grams of fresh particles in each test, and a total of approximately 300 grams of fresh particles.

[0112] The total time (heat treatment time and test time) for testing the fresh density of each group of samples is about 6 to 13 hours.

[0113] 10 groups of fresh density The test results:

[0114] The isovalues ​​of GCBA fresh density of WBP-FA-SF ternary system can be found in Figure 3 , which reflects the physical accumulation state of the precursors in the fresh GCBA particles;

[0115] It can be seen that the fresh density of GCBA synthesized by the WBP-FA-SF ternary system is between 0.55 and 0.72;

[0116] Specifically, within the composition range of about 45-80 vol% of waste brick powder (WBP) and 10-20 Vol% of silica fume (SF), the fresh density of fresh particle samples was higher (0.68-0.72);

[0117] When the ratios of WBP, FA and SF are 75 vol%, 12.5 vol% and 12.5 vol% respectively, the fresh density is the highest at 0.72, which indicates that the solid precursor particles in the fresh GCBA particles form the densest physical stacking state at this time.

[0118] (7) Optimization, solidification and screening of GCBA

[0119] The precursor formula corresponding to the highest fresh density of 0.72 was selected as the preferred group, and the other 9 groups were selected as the control group.

[0120] The above 10 groups of fresh granules synthesized by the disc granulator were first placed in a constant temperature oven at 80°C for 24 hours of constant temperature heat curing, and then sealed at room temperature to continue curing for 28 days.

[0121] After solidification, particles with a particle size of 4.75 to 9.5 mm were screened out as the final GCBA;

[0122] 10 different combinations of GCBA samples are available at Figure 4 .

[0123] (8) Hardening strength of the preferred group GCBA

[0124] After curing (thermal curing for 1 day + room temperature curing for 28 days), compared with the other 9 groups of control GCBA, the preferred group GCBA showed the highest cylinder pressure strength (42.2MPa) and the highest single particle strength (20.21MPa). This shows that by selecting the fresh GCBA particles with the highest fresh density, the GCBA particles with the highest strength can be synthesized after curing.

[0125] (9) Synthesis cost of preferred group GCBA

[0126] Compared with the other 9 groups of control GCBA, the preferred group GCBA showed the lowest liquid-solid ratio (0.17). This shows that after the fresh particles are optimized for the highest fresh density, the lowest GCBA base activator solution dosage can be achieved, thereby achieving the lowest GCBA synthesis cost.

[0127] (10) Reaction degree of the preferred group GCBA

[0128] After curing (thermal curing for 1 day + room temperature curing for 28 days), the preferred group GCBA showed the lowest reaction degree (8.1%) compared with the other 9 control groups, which indicates that after the fresh GCBA particles are optimized for the highest fresh density, only a lower reaction degree (fewer reaction products) is required to cure to form a higher strength GCBA.

[0129] (11) Application of GCBA in ultra-high performance concrete

[0130] The preferred group GCBA was used to produce ultra-high performance concrete according to the mix ratio in Table 3.

[0131] Table 3

[0132]

[0133] Then, the fresh UHPC mixture was poured into a mold with a size of 50 mm × 50 mm × 50 mm and compacted on a vibration table; then, the specimen covered with plastic film was demoulded after being stored at room temperature for 15 h;

[0134] After demoulding, the UHPC specimens were cured in a steam curing box at 80°C for 48 hours. The heating and cooling rates during the steam curing process were both 12°C / hour. The steam-cured specimens were transferred to a standard curing box and continued to be cured until the 7th day.

[0135] The 7-day compressive strength of UHPC containing the preferred group GCBA was tested with reference to T / CECS864-2021, and the result was as high as 162.9 MPa.

[0136] In summary, by combining (5)-(7) in Example 1, it can be seen that the performance optimization method based on fresh density proposed in the present invention has significant advantages of efficient and fast testing, extremely short optimization cycle, minimal consumables required for optimization, and time-saving and labor-saving optimization process;

[0137] By combining (7)-(10) in Example 1, it can be seen that the GCBA selected based on the highest fresh density can simultaneously have the highest strength and the lowest cost, and only requires the lowest degree of reaction to synthesize the highest strength geopolymer-free sintering artificial aggregate;

[0138] It can be seen from (11) in Example 1 that the GCBA selected based on the highest fresh density is suitable for use in ultra-high performance concrete above 150 MPa.

[0139] Example 2

[0140] The purpose of this example is to illustrate that the performance optimization method based on fresh density can simultaneously achieve strength improvement and cost reduction of GCBA.

[0141] Figure 5 The relationship between the fresh density, cylinder pressure strength and liquid-solid ratio of the 10 groups of GCBA in Example 1 is shown. It can be seen that as the fresh density increases from 0.55 to 0.72, the cylinder pressure strength increases from 11.4 MPa to 42.2 MPa, an increase of 270%; while the liquid-solid ratio decreases from 0.33 to 0.17, a decrease of 52%.

[0142] As mentioned in the technical background, the cost of the alkaline activator solution accounts for about 80% of the total synthesis cost. Therefore, this means that as the fresh density increases from 0.55 to 0.72, the strength of GCBA increases by about 270%, while the synthesis cost decreases by about 40%.

[0143] Example 3

[0144] The purpose of this example is to illustrate that the performance optimization method based on fresh density can be a physical enhancement method that can synthesize higher strength artificial aggregates through mix proportions with lower reaction degrees.

[0145] See the contour diagram of the reaction degree of the ternary system GCBA hardened particles in Example 1. Figure 6 ;

[0146] See the cylinder compressive strength contour diagram of the ternary system GCBA hardened particles in Example 1. Figure 7 ;

[0147] See the fresh density contour diagram of the ternary system GCBA hardened particles in Example 1. Figure 3 ;

[0148] like Figure 6 As shown, the reaction degree of GCBA is only about 8-13%, which is significantly lower than the typical range of 40-60% reported for geopolymer cast-in-place paste materials (such as geopolymer concrete, geopolymer mortar, and geopolymer paste).

[0149] The main reason for this difference is that the GCBA of the present invention uses a smaller amount of alkaline activator solution.

[0150] from Figure 6 It can also be seen that within the composition range of about 45-80 vol% WBP and about 10-20 vol% SF, the reaction degree of GCBA is slightly lower (about 8-9%).

[0151] Sample 75W-12.5F-12.5S showed the lowest degree of reaction, only about 8.1%.

[0152] In the combined region of 45-70 vol% WBP and 30-50 vol% SF, the reaction degree of GCBA was relatively high (about 10-12.8%).

[0153] Will Figure 6 The degree of reaction combined Figure 3 From the fresh density results shown, it seems that high reaction levels tend to appear in samples with low fresh density, while low reaction levels appear in samples with high fresh density. This is because the increase in fresh density leads to a decrease in the amount of alkaline activator solution (e.g. Figure 5 As shown in the figure, since the reaction degree of GCBA is affected by the amount of base activator, the less the amount of base activator, the lower the reaction degree.

[0154] Traditionally, the strength of geopolymer concrete, mortar or paste is positively correlated with its degree of reactivity; however, the opposite phenomenon is observed in GCBA.

[0155] Will Figure 6 The degree of reaction combined Figure 7 From the cylinder pressure strength results shown, the sample with the highest strength (75W-12.5F-12.5S, cylinder pressure strength 42.2MPa) has the lowest reaction degree (8.1%); while the reaction degree of the GCBA with lower strength is relatively high. For example, the reaction degree of sample 45W-5F-50S is the highest among the 10 groups of GCBA (12.8%), but the corresponding strength is relatively low (cylinder pressure strength 11.4MPa).

[0156] The results of the cylinder pressure strength, fresh density and reaction degree of GCBA are summarized ( Figure 7 , Figure 3 , Figure 6), it can be seen that the beneficial effect of the increase in fresh density on the strength of GCBA is far greater than the adverse effect of the decrease in reaction degree on the strength.

[0157] Therefore, at higher fresh density, the strength of GCBA can be significantly improved even with a reduced degree of reaction.

[0158] Therefore, it can be proved that improving the fresh density is a physical reinforcement method for geopolymer unfired artificial aggregate, which can synthesize higher strength artificial aggregate at a lower reaction degree.

[0159] Example 4

[0160] The purpose of this example is to illustrate the effect of the proposed performance optimization method on improving the strength of GCBA, and to compare the strength of the optimized GCBA aggregate in Example 1 with the domestic and international levels of artificial aggregate strength and the strength of natural pebbles.

[0161] (1) Improvement effect

[0162] For the 10 groups of artificial aggregates in Example 1, Figure 8 As shown in the figure, as the fresh density increases from 0.55 to 0.72, the cylinder compressive strength increases from 11.4 MPa to 42.2 MPa, an increase of 270%, showing an exponential growth trend. This shows that the physical enhancement method based on fresh density has a significant effect on improving the strength of artificial aggregate.

[0163] (2) Comparison of strength levels of artificial aggregates at home and abroad

[0164] Domestic level: In Example 1, the cylinder compressive strength of the GCBA selected after the highest fresh density is 42.2MPa, which is 549% higher than the strength index of the high-strength artificial aggregate with the highest strength grade specified in the national standard "GBT 17431.1-2010 Light aggregate and its test method Part 1: Light aggregate" (strength grade 40, cylinder compressive strength 6.5MPa).

[0165] International level: In Example 1, the single particle strength of GCBA selected after the highest fresh density is 20.21MPa, which is compared with the single particle strength of 72 kinds of artificial aggregates collected in international review literature. It is worth mentioning that the above 72 kinds of artificial aggregates include various types of artificial aggregates including sintered and non-sintered ones, representing the international level of artificial aggregate strength.

[0166] like Fig. 9As shown, the strength of most artificial aggregates reported internationally hovers below 12MPa, especially unsintered artificial aggregates. The single particle strength (20.21MPa) of GCBA developed by optimally developing the highest fresh density in Example 1 exceeds the strength level of most artificial aggregates including sintered and unsintered aggregates reported internationally, reaching the international leading level.

[0167] in, Fig. 9 The literature represented by [1] is:

[0168] P.-F.Ren,T.-C.Ling,KHMo,Recent advances in artificial aggregate production,Journal ofCleaner Production.291(2021),125215.https: / / doi.org / 10.1016 / j.jclepro.2020.125215

[0169] (3) Comparison with natural pebbles

[0170] In Example 1, the cylinder compressive strength of the GCBA selected after the highest fresh density is 42.2 MPa, which is about 40% higher than the cylinder compressive strength of natural pebbles with the same particle size range of 28-30 MPa.

[0171] In summary, the physical reinforcement method based on fresh density has a very significant effect on improving the strength of artificial aggregate. The strength of the GCBA developed in this way is even higher than that of natural pebbles, reaching the international leading level of artificial aggregate strength.

[0172] Example 5

[0173] The purpose of this example is to illustrate the effect of fresh density on the microstructure of GCBA after curing:

[0174] With the increase of fresh density, the microstructure of cured GCBA was significantly densified and homogenized, although the reaction products of cured GCBA were reduced.

[0175] Next, the GCBA sample (90W-5F-5S) with a fresh density of 0.63 and the GCBA sample (75W-12.5F-12.5S) with a fresh density of 0.72 in Example 1 were selected for microstructural characterization and comparative analysis to prove the above point of view.

[0176] Fig.10 The microstructure of the two GCBA samples is shown. The microstructure of the GCBA sample (90W-5F-5S) with a fresh density of 0.63 is a granular porous structure ( Fig.10 (a)). In contrast, the microstructure of the GCBA sample (75W-12.5F-12.5S) with a fresh density of 0.72 is more uniform and dense ( Fig.10 (b)).

[0177] Their pore structures are Fig.11 As shown in Table 4:

[0178] Compared with the GCBA sample (90W-5F-5S) with a fresh density of 0.63, the porosity of the GCBA sample (75W-12.5F-12.5S) with a fresh density of 0.72 is obviously lower ( Fig.11 (b)), and the average pore size was reduced by 41.55%, especially for pores larger than 1 μm (Table 4).

[0179] Table 4

[0180]

[0181] In summary, the pore structure of the solidified particles can be regulated and optimized by regulating and optimizing the physical stacking state of the precursor of fresh GCBA particles through fresh density.

[0182] Example 6

[0183] The purpose of this example is to demonstrate that ultra-high strength artificial aggregate based on physical enhancement of fresh density can be used to produce ultra-high performance concrete with a compressive strength of more than 150 MPa.

[0184] (1) Mixing ratio, production process and testing of ultra-high performance concrete (UHPC)

[0185] From Example 1, a GCBA (75W-12.5F-12.5S, fresh density 0.72, cylinder pressure strength 42.2 MPa) that was selected for the highest fresh density and a common GCBA (90W-5F-5S, fresh density 0.62, cylinder pressure strength 17.7 MPa) that was not selected for the highest fresh density were selected as coarse aggregates for preparing two types of UHPC, respectively referred to as U-HGCA and U-LGCA.

[0186] For reference and comparison, two other types of UHPC were prepared using commercial unburned aggregate (cylinder compressive strength 3.2 MPa) and natural aggregate as coarse aggregate, respectively, and were named U-CCA and U-NA.

[0187] The four types of UHPC used the same mix ratio, with the only variable being the type of coarse aggregate. The coarse aggregate content in all types of UHPC was 20 vol%, and the coarse aggregate particle size ranged from 4.75 to 8 mm.

[0188] The mass of the four types of UHPC fine aggregates (i.e., quartz sand) is 25% of the mass of the cementitious material.

[0189] The amounts of steel fiber and water reducing agent for the four types of UHPCs remained unchanged, which were 2 vol% of the total volume of UHPC and 2 wt% of the mass of cementitious materials, respectively.

[0190] Table 5 lists the mix proportions of four types of UHPC.

[0191] Table 5

[0192]

[0193] Use a vertical planetary mixer to mix fresh UHPC. The mixing process is carried out in the following steps:

[0194] 1) Dry mix the cementitious material and fine aggregate in a mixer at low speed for 3 minutes;

[0195] 2) Then pour the mixed solution of water and water reducing agent into the mixer and stir at low speed for 7 minutes.

[0196] During this process, when the mixture is fluid (approximately from the 3rd minute onwards), the steel fibers are slowly and dispersedly added to the mixer, followed by the coarse aggregate without pre-wetting;

[0197] 3) Finally, the mixture was stirred at high speed for another 2 minutes.

[0198] Then, the fresh UHPC mixture was poured into a mold with the size of 50 mm × 50 mm × 50 mm and vibrated on a vibration table to remove air bubbles;

[0199] Then, the specimen covered with plastic film was stored at room temperature for 15 hours and then demoulded;

[0200] After demolding, the concrete specimens were cured in a steam curing machine at 80°C for 48 hours. The heating and cooling rates during the steam curing process were both 12°C / hour. The steam-cured specimens were transferred to a standard curing box at 20°C and 95% humidity and continued to be cured until the 7th day.

[0201] Before the strength test, these UHPC specimens were dried in an oven at 70 °C for 12 h to remove moisture from the surface of the specimens.

[0202] The test procedure for the 7-day compressive strength of ultra-high performance concrete shall be carried out in accordance with T / CECS864-2021.

[0203] (2) UHPC compressive strength test results

[0204] Fig.12The compressive strength test results of four concrete samples produced with four coarse aggregates are shown. It can be seen that the strength of the concrete sample U-HGCA containing the preferred GCBA with the highest fresh density (75W-12.5F-12.5S) is as high as 162.9MPa, which is only 9.7% lower than the strength of UHPC using natural coarse aggregate (U-NA, 180.3MPa). In addition, the strength of the concrete sample U-LGCA containing ordinary GCBA (90W-5F-5S) is 131.1MPa, which is lower than that of U-HGCA containing the preferred GCBA with the highest fresh density. It is worth mentioning that among the concretes produced with the above three artificial coarse aggregates (U-CCA, U-LGCBA, U-HGCA), only the concrete produced with the preferred GCBA with the highest fresh density reaches the compressive strength index of ultra-high performance concrete (UHPC) (higher than 150MPa).

[0205] Compared with U-CCA containing commercial unburned artificial aggregate and U-LGCA containing ordinary GCBA, the strength of U-HGCA containing GCBA selected with the highest fresh density is significantly improved by 49.9% and 24.3%, respectively.

[0206] These results confirm that geopolymer-free sintering artificial aggregate based on physical enhancement of fresh density can be suitable for the production of ultra-high performance concrete above 150 MPa, which represents an advanced strategy for high-value recycling of solid waste.

[0207] Example 7

[0208] The purpose of this example is to emphasize the technical advantages of the performance optimization method based on fresh density in that the optimization process takes very little time and the sample preparation is simple.

[0209] Regarding the test of fresh density, the total amount of fresh particle samples required for each group is 250-300 ml (bulk volume), which can meet the total amount of samples required for three parallel tests;

[0210] The test of fresh density of each group is divided into two stages: heat treatment and test. The heat treatment stage requires 5 to 15 hours, and the average test stage requires 0.5 hours, that is, the total time is 6 to 16 hours per group; the temperature required in the heat treatment stage is 40 to 80°C.

[0211] Fresh density is the volume V of the precursor in the fresh particle P The apparent volume V of fresh particles F The ratio is:

[0212]

[0213]

[0214] In the formula, m p and m F represent the mass of solid precursor in fresh particles and the mass of fresh particles, respectively; LSR represents liquid-solid ratio; represents the precursor material; ρ x represents the absolute density of the solid precursor component x; VR x Represents the volume ratio of precursor component x to the solid precursor mixture, satisfying:

[0215]

[0216] Fresh particle apparent volume V F It can be measured by Archimedes drainage method on fresh particles treated with heat (pre-treatment);

[0217] Among them, when the heat treatment (pretreatment) time is less than 1 to 5 hours, or the heat treatment temperature is lower than 40°C, the fresh particles may dissolve in the water and the particle volume cannot be measured by the Archimedes drainage method;

[0218] When the heat treatment time is longer than 15 h, or the heat treatment temperature is higher than 80 °C, the particle volume measured by the water displacement method will be different from the apparent volume V of the fresh particles. F There may be large deviations.

[0219] Therefore, the present invention preferably selects 5 to 15 hours and 40 to 80°C as the heat treatment (pretreatment) system for testing the fresh density, which ensures that the particles after heat treatment maintain their original shape in water and will not dissolve in water, and that the measured particle volume is basically the same as the apparent volume of the actual fresh particles (the theoretical volume deviation is less than 1.0%, so it can be ignored).

[0220] As we all know, hardened artificial aggregates are composed of two major parts: solid and pores. The reduction of pores (or the increase of density) is the reason for the increase in strength. The solid part is composed of reaction products and unreacted raw material particles. The existing technology still mainly relies on chemical enhancement to improve the performance of geopolymer artificial aggregates, such as using highly active raw materials and high-dose and high-concentration alkali activators. Although the proportion of reaction products can be increased to improve the density after hardening, this undoubtedly causes a huge cost burden that cannot be ignored.

[0221] In contrast, the fresh density method proposed in the present invention is a physical reinforcement method. First of all, the most significant improvement of this new method over existing chemical reinforcement methods is that it can achieve both strength improvement and cost reduction. Specifically, the motivation of the fresh density method is to improve the packing density of the unreacted raw material particles inside the artificial aggregate in the initial granulation stage (fresh stage), thereby improving the density of the artificial aggregate after hardening, and ultimately achieving an increase in hardening strength; in addition, due to the increase in the density of the unreacted particles, the artificial aggregate only needs less reaction products to achieve the densification of the hardened particles, which means that a lower dose or concentration of the alkali activator is allowed to be used, ultimately achieving cost reduction, because the alkali activator is the main source of cost of geopolymer artificial aggregate (accounting for 80% or more). In summary, the primary improvement of the present invention over existing reinforcement technology is that it can simultaneously achieve both strength improvement and cost reduction of geopolymer artificial aggregate.

[0222] Secondly, compared with the existing optimization technology based on the hardening performance of GCBA, the GCBA optimization technology based on fresh density proposed in the present invention has the significant advantages of high efficiency and convenience. Specifically, the existing optimization procedure of GCBA is based on the hardening performance of GCBA, and obtaining the hardening performance of GCBA usually requires a long time period of more than 28 days and time-consuming; in contrast, the performance optimization method proposed in the present invention is based on fresh density, and the time period for evaluating the fresh density of artificial aggregate only takes less than 16 hours, which is significantly shorter than the 28 days generally required for evaluating hardening performance in the prior art. In addition, evaluating the hardening performance (such as cylinder pressure strength, water absorption, apparent density, and bulk density) of a group of artificial aggregates conservatively requires at least 5 liters of samples, while evaluating the fresh density of a group of artificial aggregates only requires about 300 milliliters of samples. Therefore, the optimization method based on fresh density proposed in the present invention can greatly shorten the time-consuming optimization of artificial aggregate performance, and can greatly reduce the trial and error cost and cumbersome sample preparation work, which is more efficient and fast.

[0223] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A physical reinforcement method for geopolymer sinter-free artificial aggregate based on fresh density, Features: include, The solid precursor powder of the geopolymer unburned artificial aggregate is added into a disc granulator, and the alkaline activator solution is evenly sprayed on the powder in a mist form until the fine particles are wrapped into fresh particles of the geopolymer unburned artificial aggregate of the required diameter; Testing the fresh density of fresh particles, and selecting the solid precursor formula with the highest fresh density; The fresh particles prepared by using the preferred formula are solidified and sieved to obtain the sinter-free artificial aggregate based on physical reinforcement geopolymer; Among them, fresh density is the volume V of the solid precursor in the fresh particles P The apparent volume V of fresh particles F The ratio is: In the formula, m p and m F represent the mass of the solid precursor in the fresh particles and the mass of the fresh particles, respectively; LSR represents the liquid-solid ratio, that is, the ratio of the mass of the alkaline activator solution to the mass of the solid precursor in the fresh particles; represents the solid precursor material; ρ x represents the absolute density of the solid precursor component x; VR x Represents the volume ratio of the solid precursor component x to the solid precursor mixture, satisfying: Fresh particle apparent volume V F The fresh particles are placed in a 40-80℃ oven for constant temperature heat treatment for 5-15h, and then measured by the Archimedes drainage method after cooling; Among them, the test of fresh density includes two stages: heat treatment and testing. The heat treatment stage requires 5 to 15 hours, the average testing stage requires 0.5 hours, and the total time is 6 to 16 hours; the temperature in the heat treatment stage is 40 to 80°C.

2. The method according to claim 1, Features: The solid precursor powder of the fresh particles includes a powder rich in silicon and aluminum components and a solid waste powder with alkali excitation activity or low alkali excitation activity, wherein the powder rich in silicon and aluminum components includes fly ash and silica ash, and the solid waste powder with alkali excitation activity or low alkali excitation activity includes one or more of waste brick powder, red mud powder, waste ceramic powder, waste glass powder, rice husk ash powder, biomass fly ash, lithium slag powder, waste stone powder, concrete recycled micropowder, residual mud powder, engineering slag powder, silt powder, steel slag powder, municipal waste incineration furnace slag powder, and municipal waste incineration fly ash.

3. The method according to claim 1 or 2, Features: The maximum particle size of the solid precursor powder used for disc granulation is less than 175 μm, and the particle size dv90 of 90 vol% cumulative proportion is less than 75 μm; the solid precursor powder used for disc granulation is in a dry state.

4. The method according to claim 1 or 2, Features: The solid precursor powder of the fresh particles, wherein the powder rich in silicon and aluminum components accounts for 20-50 vol%, and the solid waste powder accounts for 50-80%; the liquid-to-solid ratio of the fresh particles is 0.12-0.

35.

5. The method according to claim 1, Features: The alkali activator solution comprises one of potassium water glass and sodium water glass, wherein the modulus of potassium water glass is 0.9-1.4, the mass concentration is 25%-45%, and the modulus of sodium water glass is 0.8-1.2, the mass concentration is 25%-35%.

6. The method according to claim 1, Features: The fresh density test, wherein the fresh particles after heat treatment have the ability to maintain their original shape in water and not dissolve in water.

7. The method according to claim 1, Features: The curing comprises two stages: thermal curing at 40-80°C for 10-24 hours and subsequent natural curing at room temperature for more than one day; the screening comprises screening the cured artificial aggregate particles through a sieve with a size range of 2.36-9.5 mm.

8. The high-strength geopolymer sinter-free artificial aggregate prepared by the method according to any one of claims 1 to 7, Features: The liquid-to-solid ratio of fresh particles obtained by the preferred formula is lower than 0.18, the fresh density is higher than 0.68, the reaction degree of the aggregate after solidification is lower than 10%, and the strength of the aggregate after solidification is higher than that of natural pebbles.

9. The geopolymer sinter-free artificial aggregate according to claim 8 is suitable for use in ordinary concrete, high-strength concrete and ultra-high performance concrete.

Citation Information

Patent Citations

  • Self-compacting concrete and preparation method thereof

    CN112707685A

  • Preparation method of geopolymer sintering-free artificial aggregate and application of geopolymer sintering-free artificial aggregate in high-strength concrete

    CN113998934A

  • Geopolymer precursor powder convenient for site construction, preparation method and construction method

    CN117623655A

  • Performance-enhancing particulate premix comprised of mineral fines treated with one or more additives

    US20240174565A1

  • Building waste burn-free regeneration brick and preparation method thereof

    WO2022062493A1