Sludge soft soil reinforcing layer for near-water excavation deep foundation pit support and forming construction method
By using cement slurry, fume, nanosilica, talc powder and premature water reducing agent in sludge soft soil for deep stirring and spraying technology, the low strength and high permeability of sludge soft soil layer is solved. The problem of efficiency and environmental protection has achieved efficient and environmentally friendly reinforcement effect, meeting the construction needs of the deep foundation pit of the main pier of the bridge.
Patent Information
- Application Number
- CN202410944548.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-26
AI Technical Summary
Under the conditions of silt soft soil layers with high moisture content, large pore ratio and low bearing capacity, how to prepare reinforced layers with high strength, early strength, high bearing capacity and good water stopping performance to ensure the depth of the main pier of the bridge to ensure the bearing of the main pier of the bridge Safety and environmental protection of foundation pit construction.
The cement slurry composed of cement, silica fume, nano silica, talc powder and premature water reducing agent are mixed with sludge soft soil. Through deep mixer mixing and spraying technology, the pores between soil particles are filled and the pores are quickly condensed to form high Density, early strength type silt soft soil reinforcement layer.
The high strength, early strength, good water stop performance and low construction cost of the silt soft soil reinforcement layer are achieved, the strength and stability requirements of deep foundation pit support are met, construction pollution is avoided, and construction period is shortened.
Smart Images

Figure BDA0004945238100000161 
Figure BDA0004945238100000201 
Figure BDA0004945238100000221
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of soft soil reinforcement construction, in particular to a silty soft soil reinforcement layer and a molding construction method for supporting a deep foundation pit excavated near water. Background Art
[0002] In a bridge project in the Guangdong Delta Plain, the bridge 7# main pier cap passes through the silty clay layer, medium sand layer, silty silty sand layer, and silty silty clay layer, and is located on the silty silty clay layer. The natural moisture content of the soil layer in the construction site of the bridge 7# main pier cap is 28.7~49.5%, the water saturation is 88.3~99.0%, the porosity is 0.790~1.319, the foundation bearing capacity is 50~220kPa, the direct quick shear cohesion is 3.8~14.8kPa, and the internal friction angle is 2.3°~13.7°. It has high moisture content, large porosity, low bearing capacity, and low shear strength. The physical and mechanical properties of the soil are poor, the geological conditions are poor, and the lateral support force for the foundation pit cofferdam of the bridge 7# main pier cap is small. It is very easy to overturn or slide, and unconventional foundation pit support is required. Common types of foundation pit supports include: pile support, pile brace, pile anchor, pile cantilever, underground continuous wall support, ground-anchored wall + support, cement retaining wall, soil nail wall (sprayed anchor support), reverse arch wall, original soil slope, pile, wall and support system, simple horizontal support, reinforced concrete pile row and other forms.
[0003] Based on the location of the bridge's 7# main pier cap near the secondary water source Meixi River, which is about 3m away, in order to prevent the construction sewage in the cap foundation pit from infiltrating into the nearby river outside the foundation pit through the pores between the stratum soil particles, polluting the river water quality, or the groundwater outside the cap foundation pit from infiltrating into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier cap, the silty soft soil reinforcement layer is designed with early strength and water stopping requirements of 3d unconfined compressive strength ≥ 0.8MPa. Based on the fact that the cap foundation pit is a 7.5m deep foundation pit excavated near the water, in order to prevent the cap foundation pit soil from easily overturning or sliding after the cap foundation pit is excavated due to the low strength and small lateral support force of the silty soft soil reinforcement layer, the deep foundation pit support strength, bearing capacity and lateral support force requirements of 28d unconfined compressive strength ≥ 1.0MPa are designed for the silty soft soil reinforcement layer.
[0004] Therefore, when constructing the deep foundation pit of the 7# main pier cap under the soil conditions of "high water content, large porosity, low bearing capacity and low shear strength", how to prepare a silty soft soil reinforcement layer with high strength, early strength, high bearing capacity and good water-stopping performance will be an urgent problem to be solved in the safe construction of the deep foundation pit support of the 7# main pier cap of the bridge. Summary of the invention
[0005] The present invention provides a silty soft soil reinforcement layer and a molding construction method for supporting deep foundation pits excavated near water, so as to solve the technical problems of difficulty in molding the silty soft soil layer, high permeability, poor water-stopping performance, low strength, low bearing capacity, small lateral supporting force, poor foundation pit stability and pollution of river water quality during construction. The invention has the beneficial effects of simple construction process operation, short construction period, low construction cost and environmental protection.
[0006] According to one aspect of the present invention, a silty soft soil reinforcement layer for supporting deep foundation pits excavated near water is provided, wherein the reinforcement layer comprises a reference material and cement slurry; the reference material is silty soft soil, and the cement slurry comprises cement, silica fume, nano-silicon dioxide, talcum powder, early strength water reducing agent and mixing water; the mass ratio of cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 275-325:22-26:2.75-3.25:13.75-16.25:4.13-4.88:178-180;
[0007] The silty soft soil and cement slurry are mixed in a volume ratio of 1:0.27-0.33.
[0008] Furthermore, the reference material is silty soft soil prepared by mixing silty clay, medium sand, silty silt sand, and silty silty clay in a blending ratio of 10%:11%:9%:70% of the stratum thickness.
[0009] Furthermore, the reference material and cement slurry are mixed in a volume ratio of 1:0.28-0.30.
[0010] Furthermore, the mass ratio of cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 296-300: 23.61-24.06: 2.96-3.00: 14.76-15.04: 4.43-4.51: 178-180.
[0011] Furthermore, the mass ratio of cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 298:23.84:2.98:14.90:4.47:179.
[0012] Furthermore, the silty soft soil passes through a 5 mm sieve.
[0013] According to another aspect of the present invention, there is also provided a method for forming a silty soft soil reinforcement layer for supporting a deep foundation pit excavated near water, comprising the following steps:
[0014] S1: Set up a cement slurry mixing station and a storage tank near the silty soft soil layer to be reinforced at the construction site. After the cement slurry is mixed, the cement slurry is pumped into the grouting pipe of the deep mixer by the slurry hose; connect the slurry hose with the storage tank, mortar pump and deep mixer, start the deep mixer, and use the deadweight of the deep mixer to vertically sink the drill rod at a uniform speed of 0.3-0.5m / min to the designed reinforcement depth. While sinking, spray and stir at a uniform speed of 0.3-0.5m / min; when the drill rod enters 0.5m from the top surface of the silty soil layer, start the mortar pump, and continuously press the cement slurry from the central pipe of the deep mixer into the silty soil layer. The cement slurry and the silty soil layer are mixed by the mixer's mixing blades, and the slurry is sprayed while mixing until the designed reinforcement depth is reached;
[0015] S2: After the deep mixer sinks to the designed reinforcement depth and mixes and sprays at the end of the cylindrical pile, it is mixed and lifted at a uniform speed of 0.3-0.5m / min, and cement slurry is sprayed at the same time. The cement slurry is continuously pressed into the silty soil layer from the central tube of the deep mixer. The cement slurry and the silty soil layer are mixed by the mixing blades of the mixer. The slurry is sprayed while mixing until it is 0.5m away from the top surface of the silty soil layer. The spraying is stopped, and the mixing process is completed once;
[0016] S3: Each cylindrical pile must be re-mixed to obtain a reinforced layer formed cylindrical pile.
[0017] Furthermore, the grouting pressure of the cement slurry is 0.40MPa to 0.60MPa.
[0018] Furthermore, in step S3, the re-stirring is performed four times and four times for each cylindrical pile, and the speed of the first sinking stirring and the lifting stirring is 0.3 or 0.4 m / min; during the re-stirring, the sinking stirring is performed at a speed of 0.4 or 0.5 m / min, and the lifting stirring is performed at a speed of 0.3 or 0.4 m / min, and there is a short pause between the two stirrings.
[0019] Furthermore, in step S3, the normal forming time of each cylindrical pile is not less than 40 minutes, and the shotcrete pressure is not less than 0.4 MPa.
[0020] The present invention has the following beneficial effects:
[0021] 1. The present invention adopts silty soft soil as the reference material of the silty soft soil reinforcement layer to construct the skeleton structure of the silty soft soil reinforcement layer; cement, silica fume, nano-silicon dioxide, talcum powder, early strength water-reducing agent and mixing water are sprayed and pressed into the silty soft soil to prepare a cement slurry with high density, good fluidity, strong injectability and early strength; the silty soft soil reinforcement layer is formed by stirring, squeezing and filling the pores between the silty soft soil particles with a deep mixer, and quickly solidifying.
[0022] 2. The present invention achieves the following effects by adjusting the mass ratio of the components of the cement slurry and the volume ratio of the muddy soft soil to the cement slurry:
[0023] 1) Cement consumption is saved by 7-57kg / m 3 On the basis of cement silt soft soil, silica fume, nano silicon dioxide, talcum powder and early strength water reducing agent are added to promote the rapid coagulation of cement silt soft soil to form a high-strength, early-strength silt soft soil reinforcement layer, which can not only meet the strength requirements of the deep foundation pit support of the bridge 7# main pier cap facing the water, but also save cement consumption and reduce the construction cost of the silt soft soil reinforcement layer.
[0024] 2) The cement slurry density increased by 0.03-0.16 g / cm 3 . Silica fume, nano-silicon dioxide, talcum powder and early strength water reducing agent are added to ordinary cement slurry (i.e. composed of cement and mixing water) to obtain high-density and early-strength cement slurry. The pores between the silty soft soil particles are stirred, squeezed and filled by a deep mixer to improve the density and mechanical properties of the silty soft soil layer, thereby improving the bearing capacity and lateral support force of the silty soft soil reinforcement layer.
[0025] 3) The fluidity of cement slurry is reduced by 3.2 to 6.5 seconds. In ordinary cement slurry (i.e. composed of cement and mixing water), silica fume, nano-silicon dioxide, talcum powder, and early strength water-reducing agent are added to obtain cement slurry with good fluidity, strong injectability, and early strength, which promotes the rapid and smooth injection and continuous injection of cement slurry into the silty soft soil layer, so that the silty soft soil and cement slurry are evenly mixed, and the homogeneity and overall consolidation of the silty soft soil reinforcement layer are improved.
[0026] 4) The initial setting time is shortened by 12-27 minutes, and the final setting time is shortened by 17-25 minutes. On the basis of cement muddy soft soil, silica fume, nano-silicon dioxide, talcum powder, and early strength water reducing agent are added to accelerate the hardening rate of cement muddy soft soil, so that cement muddy soft soil quickly loses plasticity from the flowing state to the solid state to form early (2-24h) solidification strength, quickly close the pores between the muddy soft soil particles, block the free flow of groundwater or construction sewage in the pores between the muddy soft soil particles, and improve the water-stopping performance of the muddy soft soil reinforcement layer; prevent the construction sewage in the foundation pit from infiltrating into the nearby river outside the foundation pit through the pores between the stratum soil particles, polluting the river water quality, or prevent the groundwater outside the foundation pit from infiltrating into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation.
[0027] 5) The 3d unconfined compressive strength increased by 0.57-0.67MPa, and the 28d unconfined compressive strength increased by 0.32-0.47MPa. On the basis of cement muddy soft soil, silica fume, nano-silicon dioxide, talcum powder, and early strength water reducer were added to make the 3d unconfined compressive strength of the muddy soft soil reinforcement layer reach the design requirement of 28d unconfined compressive strength (i.e. ≥1.0MPa), quickly improve the bearing capacity and lateral support force of the muddy soft soil reinforcement layer, effectively shorten the maintenance age of the muddy soft soil reinforcement layer, excavate the foundation pit in advance, shorten the construction period of the foundation, and reduce construction costs.
[0028] 3. According to the Engineering Geological Survey Report of this bridge, the detailed exploration drilling hole stratigraphic data of the 7# main pier cap, and the test results of silty clay, medium sand, silty silt sand, and silty silty clay, it can be known that the soil structure of each stratum in the silty soft soil has the characteristics of "high water content, large porosity, low bearing capacity, and low shear strength". In view of the above characteristics of the soil structure of each stratum in the silty soft soil, this application adopts the following technical solutions:
[0029] (1) In the construction site of the bridge 7# main pier foundation in this application, the natural moisture content of each layer of the silty soft soil is 28.7-49.5%, and the water saturation is 88.3-99.0%, which makes it difficult to form the silty soft soil reinforcement layer.
[0030] The problem that the moisture content of each layer of silt soft soil is high and it is difficult to form the reinforcement layer of silt soft soil. In addition to using cement and water to react to absorb part of the free water in the soil of each layer in the silty soft soil, the present application also uses silica fume and nano-silicon dioxide to react to continuously absorb the remaining free water in the soil of each layer in the silty soft soil, thereby reducing the moisture content and water saturation of the soil of each layer in the silty soft soil (water saturation refers to the ratio of the volume of liquid water contained in a unit volume of rock or soil to the total pore volume. The higher the water saturation, the more water is stored in the rock or soil), thereby changing the molding environment of the silty soft soil reinforcement layer; polycarboxylic acid early strength water reducing agent is also used to react with tricalcium aluminate (C3A) in cement to accelerate the hardening rate of cement silty soft soil; silica fume, nano-silicon dioxide and calcium hydroxide, a product of cement hydration, are also used to react to form calcium silicate gel to improve the early (2 to 24 hours) solidification strength of the silty soft soil reinforcement layer, so that the cement slurry can be more easily and quickly hardened and formed after being mixed with the soil of each layer in the silty soft soil. The invention solves the problems of high moisture content of soil in various layers of silty soft soil and great difficulty in forming the silty soft soil reinforcement layer, and realizes the rapid hardening and forming and overall consolidation of the silty soft soil reinforcement layer.
[0031] (2) In silty clay, medium sand, silty silt sand, and silty silty clay strata with a porosity ratio (pore ratio refers to the ratio of the pore volume in the soil to the volume of its solid particles) of 0.790 to 1.319, due to their large porosity ratio, their permeability is large and their water-stopping performance is poor, which increases the diffusivity of cement slurry. Especially in the medium sand strata with a porosity ratio of 1.319, groundwater or construction wastewater is more likely to flow freely in the pores between the medium sand particles, causing the construction wastewater in the foundation pit of the foundation to penetrate into the nearby river outside the foundation pit through the pores between the particles of the medium sand stratum, polluting the river water quality, or causing the groundwater outside the foundation pit of the foundation to penetrate into the foundation pit through the pores between the particles of the medium sand stratum, causing water accumulation in the foundation pit, seriously affecting the construction of the foundation of the 7# main pier.
[0032] Aiming at the problems of large porosity of soil layers in silty soft soil, large permeability and poor water-stopping performance of silty soft soil reinforcement layer. In addition to using the smaller particle size characteristics of cement, silica fume, nano-silicon dioxide and talcum powder to fill the gaps between soil particles in various layers of silty soft soil and improve the compactness and water-stopping performance of the silty soft soil reinforcement layer, this application also uses silica fume, nano-silicon dioxide and cement hydration product calcium hydroxide to produce a secondary hydration reaction to form calcium silicate gel, thereby improving the early (2 to 24 hours) setting strength of the silty soft soil reinforcement layer, and uses polycarboxylic acid early strength water-reducing agent to make the cement silty soft soil quickly lose its plasticity from a flowing state to a solid state. It forms early (2 to 24 hours) solidification strength, quickly seals the pores between the silt soft soil particles, reduces the porosity of each stratum in the silt soft soil, and improves the impermeability and water-stopping properties of the silt soft soil reinforcement layer; talcum powder is also used to improve the erosion resistance of the silt soft soil reinforcement layer, reduce the permeability of the silt soft soil reinforcement layer and the diffusion of cement slurry, improve the impermeability and water-stopping properties of the silt soft soil reinforcement layer, slow down the cracking and cracking speed of the silt soft soil reinforcement layer, and improve the crack resistance of the silt soft soil reinforcement layer. The problems of large porosity of various strata in the silty soft soil, high permeability of the silty soft soil reinforcement layer and poor water-stopping performance were solved, and the construction sewage in the foundation pit of the 7# main pier cap was prevented from infiltrating into the nearby river outside the foundation pit through the pores between the strata particles in the silty soft soil, polluting the river water quality, or the groundwater outside the foundation pit of the 7# main pier cap was prevented from infiltrating into the foundation pit through the pores between the strata particles in the silty soft soil, causing water accumulation in the foundation pit, which seriously affected the construction of the 7# main pier cap.
[0033] (3) In the construction site of the bridge 7# main pier cap in this application, the direct quick shear cohesion of each layer of soil in the silty soft soil is
[0034] 3.8~14.8kPa, internal friction angle is 2.3°~13.7°, it can be known that the shear strength of each layer of soil is low, the lateral support force for the cofferdam of the foundation pit is small, resulting in poor stability of the foundation pit, which is very easy to overturn or slide.
[0035] The invention aims to solve the problems of low shear strength of soil in various layers in silty soft soil, low bearing capacity and small lateral support force of silty soft soil reinforcement layer. In addition to using smaller particles of cement, silica fume, nano-silicon dioxide and talcum powder to fill the gaps between soil particles in various layers in silty soft soil and improve the density, unconfined compressive strength and shear strength of the silty soft soil reinforcement layer, the application also uses silica fume to increase the thermal conductivity of the silty soft soil reinforcement layer, accelerate the transfer of internal heat of the silty soft soil reinforcement layer to the soil around the cylindrical pile, reduce the internal temperature of the silty soft soil reinforcement layer, reduce the evaporation of water in the silty soft soil, ensure that the secondary hydration reaction of silica fume and nano-silicon dioxide has sufficient free water, and improve the strength of the silty soft soil reinforcement layer; the water-insoluble property of nano-silicon dioxide is also used to evenly adhere to the surface of cement slurry particles to obtain high-density cement slurry, improve the compressive strength and hardness of cement slurry, and improve the fluidity of cement slurry. The silty soft soil and cement slurry are mixed evenly to improve the homogeneity, overall consolidation and strength of the silty soft soil reinforcement layer; the filler effect of talcum powder is also used to improve the unconfined compressive strength of the silty soft soil reinforcement layer, increase the tensile strength and shear strength of the silty soft soil reinforcement layer, and reduce the deformation of the silty soft soil reinforcement layer; polycarboxylic acid early strength water-reducing agent is also used to react with tricalcium aluminate (C3A) in cement to accelerate the hydration rate of tricalcium aluminate (C3A) and the formation of water-insoluble calcium aluminate (C3A3CaSO4Ca(HO)2), accelerate the hardening rate of cement silty soft soil, make the 3d unconfined compressive strength of the silty soft soil reinforcement layer reach the 28d unconfined compressive strength design requirement, and quickly improve the bearing capacity and lateral support force of the silty soft soil reinforcement layer. The problems of low shear strength of soil in various strata in silty soft soil, low bearing capacity and lateral supporting force of the silty soft soil reinforcement layer are solved, and the bearing capacity and lateral supporting force of the silty soft soil reinforcement layer are improved, thereby improving the stability of the foundation pit.
[0036] 4. The design components of the silt soft soil reinforcement layer of the present application, in addition to being used in deep foundation pit support projects near water excavation to improve the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer, can also be used according to the purpose of the engineering construction, using the same cement slurry components, by adjusting the mass ratio of each component of the cement slurry and the volume ratio of silt soft soil and cement slurry. It can be applied to the silt soft soil reinforcement construction in geotechnical engineering fields such as industrial and civil building foundations, road subgrades, river embankments and seepage prevention and protection of deep foundation pits for urban rail transit, so as to achieve the same effect of improving the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer. DETAILED DESCRIPTION
[0037] The following is a detailed description of the embodiments of the present invention, but the present invention can be implemented in many different ways as defined and covered below.
[0038] An embodiment of the first aspect of the present invention provides a silty soft soil reinforcement layer for supporting deep foundation pits excavated near water, the reinforcement layer comprising a reference material and cement slurry; the reference material is silty soft soil, the cement slurry comprises cement, silica fume, nano-silicon dioxide, talcum powder, early strength water reducer and mixing water; the mass ratio of cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducer: mixing water in the cement slurry is 275-325:22-26:2.75-3.25:13.75-16.25:4.13-4.88:178-180.
[0039] The silty soft soil and cement slurry are mixed in a volume ratio of 1:0.27-0.33.
[0040] The present invention adopts silty soft soil as the reference material of the silty soft soil reinforcement layer to construct the skeleton structure of the silty soft soil reinforcement layer; cement, silica fume, nano silicon dioxide, talcum powder, early strength water reducing agent and mixing water are sprayed and pressed into the silty soft soil to prepare a cement slurry with high density, good fluidity, strong injectability and early strength; the silty soft soil reinforcement layer is formed by stirring, squeezing and filling the pores between the silty soft soil particles with a deep mixer, and quickly solidifying. It can solve the technical problems of difficult molding of silty soft soil layers, high permeability, poor water-stopping performance, low strength, low bearing capacity, small lateral support force, poor foundation pit stability and pollution of river water quality during construction, and can achieve: saving cement consumption, reducing the construction cost of silty soft soil reinforcement layer; reducing the moisture content and water saturation of each stratum of silty soft soil; improving the homogeneity and overall consolidation of silty soft soil reinforcement layer; reducing the porosity of silty soft soil layers, improving the anti-seepage and water-stopping performance of silty soft soil reinforcement layers, and preventing construction sewage in the foundation pit from seeping through the pores between stratum soil particles. The water in the river outside the foundation pit pollutes the river water quality, or the groundwater outside the foundation pit of the cap penetrates into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier cap; the 3d unconfined compressive strength of the silty soft soil reinforcement layer reaches the design requirement of the 28d unconfined compressive strength (i.e. ≥1.0MPa), quickly improves the bearing capacity and lateral support of the silty soft soil reinforcement layer, effectively shortens the maintenance age of the silty soft soil reinforcement layer, excavates the cap foundation pit in advance, shortens the construction period of the cap, and reduces the construction cost; the technical effect of improving the stability of the cap foundation pit. It has the beneficial effects of simple construction process operation, short construction period, low construction cost and environmental protection. The design components of the silt soft soil reinforcement layer of the present application, in addition to being used in deep foundation pit support projects near water excavation to improve the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer, can also be used according to the purpose of the engineering construction, using the same cement slurry components, by adjusting the mass ratio of the various components of the cement slurry and the volume ratio of silt soft soil to cement slurry. It can be applied to silt soft soil reinforcement construction in geotechnical engineering fields such as industrial and civil building foundations, road subgrades, river embankments and seepage prevention and protection, and deep foundation pit excavation and protection of urban rail transit, so as to achieve the same effect of improving the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer.
[0041] The cement used in this application adopts Wuhu Conch brand P.O42.5 ordinary Portland cement. In the silty soft soil reinforcement layer, the addition of cement has the following effects: 1) The cementitious materials mainly composed of tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminate in the cement react chemically with the silty soft soil in the cylindrical pile and the water in the cement slurry, and gradually harden under the action of the free water in the silty soft soil to form a hard cement silty soft soil, which increases the shear strength, binding force and cohesion of the silty soft soil. 2) A thermal reaction occurs between the clinker powder and water in the cement, releasing a certain amount of water heat, causing the water in the silty soft soil to evaporate, resulting in the drying and shrinkage of the silty soft soil, further improving the strength of the silty soft soil; during the shrinkage process, the silty soft soil particles move closer to each other to form a certain particle structure, increasing the density and stability of the silty soft soil reinforcement layer. 3) The cement slurry prepared by cement, silica fume, nano-silicon dioxide, talcum powder, early strength water reducing agent and mixing water fills the gaps between the silt soft soil particles and connects with the silt soft soil particles to improve the overall consolidation of the silt soft soil reinforcement layer. 4) The high-density, fluid, injectable and early-strength cement slurry is sprayed and pressed into the silt soft soil in the cylindrical pile to increase the volume of the material in the cylindrical pile and change the cohesion and stress state of the silt soft soil; the volume of the material in the cylindrical pile is expanded, so that the connection between the silt soft soil particles is tighter, the gap between the particles is reduced, the shear strength and stiffness of the silt soft soil are increased, and the density and stability of the silt soft soil reinforcement layer are improved. 5) The surface of the cylindrical pile is rough and uneven, which forms friction with the silt soft soil around it, improves the shear strength and vertical bearing capacity of the silt soft soil reinforcement layer, resists the settlement and lateral displacement of the silt soft soil reinforcement layer, and improves the stability of the foundation pit.
[0042] The silica fume of the present application adopts SF85 grade powdered silica fume, with SiO2 content of 93.47% and specific surface area of 22.5m 2 / g, density is 2.32g / cm 3. Since silica fume has a finer fineness than cement particles, most of the particles are less than 1μm, and the average particle size is between 0.1 and 0.3μm, which is one percent of the size of cement particles. In the silty soft soil reinforcement layer, the addition of silica fume has the following effects: 1) Silica fume acts as a ball between cement particles that are approximately plate-shaped, block-shaped and have more large particles, filling the gaps between cement, reducing the use of water in cement gaps to form more free water, and is mixed with cement, nano-silicon dioxide, talcum powder, and early strength water-reducing agent to form a highly fluid cement slurry, which wraps the silty soft soil particles and fills the gaps between the silty soft soil particles, thereby improving the density and mechanical properties of the silty soft soil reinforcement layer, and reducing the permeability of the silty soft soil reinforcement layer, thereby improving the water-stopping performance of the silty soft soil reinforcement layer and preventing construction sewage in the foundation pit from passing through. The pores between the stratum soil particles penetrate into the nearby river outside the foundation pit, polluting the river water quality, or the groundwater outside the foundation pit penetrates into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation; 2) Since the main component of silica fume is SiO2, it can produce a secondary hydration reaction with calcium hydroxide, a product of cement hydration, to form calcium silicate gel, which improves the strength of silty soft soil after hardening, makes a large number of pores in the silty soft soil disappear, reduces the calcium hydroxide content, and reduces the porosity of the silty soft soil layer, thereby improving the anti-seepage performance of the silty soft soil reinforcement layer, and then improves the water-stopping performance of the silty soft soil reinforcement layer. 3) The addition of silica fume will increase the water demand, change the original water-cement ratio, and affect the performance of cement slurry. After the addition of early strength water reducer, the disadvantage of increasing the amount of water in the cement slurry and increasing the water-cement ratio of the cement slurry to meet the workability of the cement slurry after the addition of silica fume is overcome, which leads to a decrease in the unconfined compressive strength of the silty soft soil reinforcement layer. 4) Adding silica fume increases the total surface area of cement slurry aggregate and the air content in cement slurry. Tiny bubbles act as balls in cement slurry, which improves the fluidity of cement slurry. The increased bubbles increase the cohesion of silty soft soil. The bubbles adhere to the solid particles of silty soft soil, reduce the sinking of solid particles and water flow, block the seepage channel of silty soft soil, and reduce the seepage of silty soft soil reinforcement layer, thereby preventing the construction sewage in the foundation pit from infiltrating into the nearby river outside the foundation pit through the pores between the stratum soil particles, polluting the river water quality, or preventing the groundwater outside the foundation pit from infiltrating into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation. 5) Due to the increase of fine powder in cement slurry, the volume of cement slurry increases, improving the cohesiveness and water retention of cement slurry, inhibiting the seepage of silty soft soil, and thus improving the water-stopping performance of the silty soft soil reinforcement layer. 6) Since silica fume does not react easily with other substances and does not react chemically with most acids and alkalis, its particles are evenly covered on the surface of silty soft soil particles, and have strong corrosion resistance, overcoming the weak acid corrosion disadvantage of groundwater in the bridge construction site. 7) Due to the reasonable particle grading of silica fume, it can reduce and eliminate cement slurry precipitation and stratification.8) The addition of silica fume increases the thermal conductivity of the silty soft soil reinforcement layer, accelerates the transfer of heat from the internal silty soft soil reinforcement layer to the soil around the cylindrical pile, reduces the internal temperature of the silty soft soil reinforcement layer, and reduces the evaporation of water in the silty soft soil; 9) Due to the secondary hydration reaction of silica fume and nano-silicon dioxide, the excess free water in the silty soft soil is absorbed, thereby reducing the moisture content of each layer of soil in the silty soft soil.
[0043] The nano silicon dioxide of the present application adopts powdered nano silicon dioxide. Nano silicon dioxide is an amorphous white powder of 1-100nm ultrafine nanometer level, non-toxic, tasteless, pollution-free, and has a spherical microstructure, a flocculent and meshed quasi-particle structure, a molecular formula and a structural formula of SiO2, and is insoluble in water. Adding nano silicon dioxide into the silty soft soil reinforcement layer has the following effects: 1) Due to its small particle size, it fills the space not filled by cement slurry particles and hydrated substances, fills the internal pores of the silty soft soil, compacts the internal structure of the silty soft soil reinforcement layer, reduces the porosity of the silty soft soil layer, improves the compactness and mechanical properties of the silty soft soil layer, and thus improves the bearing capacity and lateral support of the silty soft soil reinforcement layer. 2) In addition to participating in the hydration reaction of the silty soft soil reinforcement layer, some active particles (such as SiO2, AI203, Fe203, etc.) can also produce secondary hydration reaction with calcium hydroxide produced by cement hydration to form calcium silicate gel. After hardening, the strength of the silty soft soil reinforcement layer is improved, and the anti-seepage performance of the silty soft soil reinforcement layer is improved, preventing the construction sewage in the foundation pit of the pedestal from infiltrating into the nearby river outside the foundation pit through the pores between the stratum soil particles, polluting the river water quality, or the groundwater outside the foundation pit of the pedestal from infiltrating into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation. 3) Due to the small size of nano-silicon dioxide particles and large specific surface area, it promotes the hydration of the muddy soft soil reinforcement layer, improves the early (2-24h) solidification strength of the muddy soft soil reinforcement layer, quickly closes the pores between the muddy soft soil particles, blocks the free flow of groundwater or construction wastewater in the pores between the muddy soft soil particles, and improves the water-stopping performance of the muddy soft soil reinforcement layer; prevents the construction wastewater in the foundation pit from infiltrating into the nearby river outside the foundation pit through the pores between the formation soil particles, polluting the river water quality, or the groundwater outside the foundation pit from infiltrating into the foundation pit through the pores between the formation soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation. 4) The surface of nano-silicon dioxide has a high active domain. After being added to the cement slurry, the hydration substances produced during the hydration process are crystal nuclei, which are preferentially deposited on the surface of the nano-particles, so that the CSH changes from a loose structure to an overall uniform and stable state, and improves the early (2-24h) solidification strength of the muddy soft soil reinforcement layer. 5) Nano-silicon dioxide in cement slurry reduces the aggregation and distribution of blocky hydrated sodium carbonate at the junction of cement slurry particles and silty soft soil particles, thereby improving the structure of the page junction area, thereby improving the fluidity and injectability of cement slurry, making the silty soft soil and cement slurry evenly mixed, and improving the homogeneity and overall consolidation of the silty soft soil reinforcement layer. 6) Since SiO2 in nano-silicon dioxide is insoluble in water, it is evenly attached to the surface of cement slurry particles to obtain high-density cement slurry, improve the compressive strength and hardness of cement slurry, improve the fluidity of cement slurry, make the silty soft soil and cement slurry evenly mixed, and improve the homogeneity, overall consolidation and strength of the silty soft soil reinforcement layer.
[0044] The talcum powder of the present application adopts white fine non-sandy powder talcum powder with a fineness of 1000 mesh (particle size of 0.015mm). In the silty soft soil reinforcement layer, the addition of talcum powder has the following effects: 1) prevent the penetration of moisture and chloride ions in the silty soft soil reinforcement layer, improve the erosion resistance of the silty soft soil reinforcement layer, reduce the permeability of the silty soft soil reinforcement layer and the diffusivity of cement slurry, improve the anti-seepage performance of the silty soft soil reinforcement layer, and then improve the water-stopping performance of the silty soft soil reinforcement layer, block the free flow of groundwater or construction sewage in the pores between the silty soft soil particles, prevent the construction sewage in the foundation pit from infiltrating into the adjacent river outside the foundation pit through the pores between the stratum soil particles, pollute the river water quality, or the groundwater outside the foundation pit of the foundation pit infiltrates into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation. 2) Add an appropriate amount of talcum powder to fill the micropores and microcracks in the cement slurry, improve the internal structure of the cement slurry, reduce the stress state, improve the fluidity of the cement slurry, mix the silt soft soil and the cement slurry evenly, and improve the homogeneity, overall consolidation and strength of the silt soft soil reinforcement layer; slow down the cracking and cracking speed of the silt soft soil reinforcement layer, thereby improving the crack resistance of the silt soft soil reinforcement layer, and overcome the disadvantages of cracking caused by the evaporation of water in the silt soft soil reinforcement layer due to the release of water heat by the cement hydration reaction, silica fume, and nano-silicon dioxide secondary hydration reaction. 3) Talc powder acts as a skeleton as a filler, reducing the construction cost of the silt soft soil reinforcement layer. At the same time, it improves the unconfined compressive strength and stability of the silt soft soil reinforcement layer, increases the tensile strength and shear strength of the silt soft soil reinforcement layer, and reduces the deformation of the silt soft soil reinforcement layer. 4) Talc powder replaces part of the cement, saves cement usage, and reduces the construction cost of the silt soft soil reinforcement layer.
[0045] The early strength water reducer of the present application adopts a polycarboxylic acid early strength water reducer. In the silty soft soil reinforcement layer, the addition of the early strength water reducer has the following effects: 1) Because its surfactant molecules are adsorbed on the surface of the particles of the silty soft soil reinforcement layer, the friction between the particles is reduced, and the electrostatic force between the particles is increased, so that the particles of the silty soft soil reinforcement layer are evenly dispersed and evenly mixed with the cement slurry, thereby improving the homogeneity and overall consolidation of the silty soft soil reinforcement layer. 2) Since the PCE molecule has a highly branched and branched structure, the hydrophilicity and hydrophobicity of the molecule are increased, forming a highly dispersed water reducer system, reducing the water-cement ratio in the cement slurry, and overcoming the disadvantage that in order to meet the workability of the cement slurry after the addition of silica fume, the amount of water in the cement slurry needs to be increased, and the water-cement ratio of the cement slurry needs to be increased, resulting in a decrease in the unconfined compressive strength of the silty soft soil reinforcement layer. 3) By adjusting the hydrophilicity-hydrophobicity ratio between particles in cement slurry, the cell pores and void ratio in cement slurry are reduced, so as to achieve the effect of reducing the water-cement ratio, thereby improving the unconfined compressive strength, bearing capacity and lateral support of the silty soft soil reinforcement layer. 4) PCE in the early strength water reducer reacts with tricalcium aluminate (C3A) in cement, accelerating the hydration rate of tricalcium aluminate (C3A) and the formation of water-insoluble calcium aluminate (C3A3CaSO4Ca(HO)2), accelerating the hardening rate of cement silty soft soil, making the 3d unconfined compressive strength of the silty soft soil reinforcement layer reach the 28d unconfined compressive strength design requirement (i.e. ≥1.0MPa), quickly improving the bearing capacity and lateral support of the silty soft soil reinforcement layer, effectively shortening the curing age of the silty soft soil reinforcement layer, excavating the foundation pit in advance, shortening the foundation construction period, and reducing construction costs. At the same time, the cement silt soft soil quickly loses its plasticity from the flowing state to the solid state to form early (2 to 24 hours) solidification strength, quickly closes the pores between the silt soft soil particles, blocks the free flow of groundwater or construction sewage in the pores between the silt soft soil particles, thereby improving the water-stopping performance of the silt soft soil reinforcement layer, and prevents the construction sewage in the foundation pit from infiltrating into the nearby river outside the foundation pit through the pores between the formation soil particles, polluting the river water quality, or the groundwater outside the foundation pit from infiltrating into the foundation pit through the pores between the formation soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier foundation. 5) In the reinforcement construction of silt soft soil, reduce the internal stress of the hardened silt soft soil reinforcement layer, make the silt soft soil reinforcement layer harder and more durable, thereby reducing the construction cost of the silt soft soil reinforcement layer and pollution to the environment.
[0046] The silty soft soil and cement slurry are mixed in a volume ratio of 1:0.27-0.33. Further, the reference material and cement slurry are mixed in a volume ratio of 1:0.28-0.30. More preferably, the reference material and cement slurry are mixed in a volume ratio of 1:0.30, thereby obtaining a reinforcement layer with higher strength at a lower cost.
[0047] In the embodiment of the present application, the reference material is made of air-dried silty clay, medium sand, silty silt, and silty silty clay, and the silty soft soil is mixed in a mixing ratio of 10%: 11%: 9%: 70% according to the stratum thickness percentage as the reference material of the silty soft soil reinforcement layer to construct the skeleton structure of the silty soft soil reinforcement layer. Further, the silty soft soil is sieved through a 5mm sieve.
[0048] The silty soft soil of this embodiment is a silty soft soil mixed with indoor silty clay, medium sand, silty silt sand, and silty silty clay according to the blending ratio of 10%:11%:9%:70% of the stratum thickness percentage, so as to simulate the soil layer to be reinforced in the project, so that the design components of the silty soft soil reinforcement layer are representative, universal and operable, which is convenient for on-site construction operation, and overcomes the problems of the reinforcement layer component design components prepared by using a single soil layer: first, the workload of the reinforcement layer component design is large, which is time-consuming, material-consuming and labor-consuming; second, there are many reinforcement layer component design components, and during the reinforcement construction, the reinforcement layer component design components of different soil layers must be frequently replaced, resulting in high replacement frequency, unstable quality and inconvenient operation; third, when deep mixing and reinforcing the soil, the drill rod of the mixer sinks downward and rises upward, and the upper soil layer must be mixed with the lower soil layer and the lower soil layer with the upper soil layer, and the reinforcement layer component design components of which soil layer cannot be replaced in time and used correctly.
[0049] In an embodiment of the present application, the mass ratio of cement: silica fume: nano-silicon dioxide: talcum powder: early strength water-reducing agent: mixing water in the cement slurry is 298:23.84:2.98:14.90:4.47:179.
[0050] The cement slurry is made by mixing cement, silica fume, nano silicon dioxide, talcum powder, early strength water reducing agent and mixing water. Among them: 1) Cement, this application uses Wuhu Conch brand P.O42.5 ordinary silicate cement, with a specific gravity of 3.06g / cm 3 Specific surface area: 377m 2 / kg, initial setting time 210min, final setting time 278min, 28-day flexural strength 7.0MPa, 28-day compressive strength 48.3MPa, its quality meets the technical requirements of P.O42.5 in the "General Portland Cement" (GB 175-2023) standard. 2) Silica fume, this application uses SF85 grade powdered silica fume, with a SiO2 content of 93.47% and a specific surface area of 22.5m 2 / g, density is 2.32g / cm 3, its quality meets the technical requirements of SF85 grade silica fume in the standard "Silica fume for mortar and concrete" (GB / T 27690-2023), and its dosage is 8% of the mass of cement. 3) Nano-silicon dioxide, this application uses powdered nano-silicon dioxide, and its dosage is 1% of the mass of cement. 4) Talc, this application uses powdered talcum powder with a fineness of 1000 mesh (particle size of 0.015mm), and its quality meets the technical requirements of general talcum powder in the standard "Talc" (GB / T 15342-2023), and its dosage is 5% of the mass of cement. 5) Early strength water reducer, this application uses polycarboxylate early strength water reducer, the main component of which is polycarboxylate (PCE), powder, its water reduction rate is 10%, and its dosage is 1.5% of the mass of cement, and its quality meets the technical requirements of water reducer in the standard "Concrete Admixture" (GB 8076-2008). 6) Mixing water: This application uses river water from the construction site. After inspection, its quality meets the requirements for concrete water in the "Standard for Water Use in Concrete" (JGJ63-2006). 7) Soft mud soil: This application uses air-dried and sun-dried silty clay, medium sand, silty silt sand, and silty silty clay that have passed a 5mm sieve, and mixes them in a ratio of 10%:11%:9%:70% to make silty soft soil. After actual measurement of 1m 3 The wet soil mass of silty soft soil is 1690kg / m when the moisture content is 49.5%. 3 .
[0051] According to another embodiment of the present invention, there is provided a method for forming a silty soft soil reinforcement layer for supporting a deep foundation pit excavated near water, comprising the following steps:
[0052] S1: A cement slurry mixing station and a storage tank are set up near the silty soft soil layer to be reinforced at the construction site. After the cement slurry is mixed, the cement slurry is pumped into the grouting pipe of the deep mixer by a slurry hose; the slurry hose is connected to the storage tank, mortar pump and deep mixer, and the deep mixer is turned on. With the help of the deadweight of the deep mixer equipment, the drill rod is vertically sunk to the designed reinforcement depth at a uniform speed of 0.3-0.5 / min. While sinking, it is sprayed and stirred at a uniform speed of 0.3-0.5m / min; when the drill rod enters 0.5m from the top surface of the silty soil layer, the mortar pump is turned on, and the cement slurry is continuously pressed into the silty soil layer from the central tube of the deep mixer at a grouting pressure of 0.40MPa-0.60MPa. The cement slurry and the silty soil layer are mixed by the mixing blades of the mixer, and the slurry is sprayed while mixing until the designed reinforcement depth; during the spraying process, the cement slurry is continuously stirred. During the grouting construction, the grouting speed shall be controlled by using a slurry flow meter, the outlet pressure of the grouting pump shall be kept at 0.40MPa~0.60MPa, and the slurry delivery speed shall be kept constant. During the grouting, an automatic grouting recorder shall be configured to record: grouting volume, drilling speed and bored pile length.
[0053] S2: After the deep mixer sinks to the designed reinforcement depth and mixes and sprays at the end of the cylindrical pile for 30 seconds, it is mixed and lifted at a uniform speed of 0.3-0.5m / min, and cement slurry is sprayed at the same time. The grouting pressure of the cement slurry is 0.40MPa-0.60MPa. The cement slurry is continuously pressed into the silty soil layer from the central tube of the deep mixer. The cement slurry and the silty soil layer are mixed by the mixer blades. The slurry is sprayed while mixing until it is 0.5m away from the top surface of the silty soil layer. The spraying is stopped, and the mixing process is completed.
[0054] S3: Each cylindrical pile must repeat the previous operation of four mixing and four spraying. The speed of the first sinking mixing and lifting mixing is 0.3 or 0.4m / min; during the re-mixing, the sinking mixing speed is 0.4 or 0.5m / min, and the lifting mixing speed is 0.3 or 0.4m / min, and a short pause is made between the two mixing. The normal molding time of each cylindrical pile is not less than 40min, and the spraying pressure is not less than 0.4MPa to obtain a reinforced layer formed cylindrical pile. The re-spraying and re-mixing method is conducive to making up for the insufficient amount of spraying at one time and accelerating the slurry reaction process.
[0055] After each cylindrical pile is mixed, the next cylindrical pile needs to be constructed using the same method and the above steps are repeated. After each day of reinforcement, the storage tank, mortar pump, deep mixer and corresponding pipelines are cleaned with clean water for reuse.
[0056] Test case:
[0057] According to the Engineering Geological Survey Report of this bridge and 7 # The strata revealed by the detailed exploration drilling holes (GSZK27 and GSZK28) where the main pier cap is located are: the strata distribution at the position of -21.59m below the ground surface are, in sequence, silty clay layer, medium sand layer, silty silt sand layer, silty silty clay layer, etc. The cap is located on the silty silty clay layer. Among them: silty clay: yellowish brown, slightly wet, plastic, thickness 1.00~4.80m, foundation bearing capacity 140kPa; medium sand: yellowish brown, saturated, medium dense, general grading, thickness 1.50~4.90m, foundation bearing capacity 220kPa; silty silt: yellowish brown, saturated, loose, general grading, thickness 1.10~3.70m, foundation bearing capacity 75kPa; silty silty clay: gray-black, saturated, plastic, partially consolidated into soft plastic, containing organic matter, relatively uniform soil, good viscosity, mixed with shell fragments and sand, thickness 10.00~28.00m, foundation bearing capacity 50kPa.
[0058] In 7 # At the construction site of the main pier foundation, an excavator was used to dig pits vertically, and samples of silty clay, medium sand, silty silt and silty silty clay were taken layer by layer. The quantity of each soil sample was no less than 1,000 kg, and the samples were stored in a sealed manner.
[0059] When taking soil samples layer by layer on site, the physical indicators, liquid limit, direct quick shear and consolidation test and other performance indicators of silty clay, medium sand, silty silt sand, and silty silty clay were tested in accordance with the standard method of "Highway Geotechnical Test Code" (JTG 3430-2020).
[0060] (1) Silty clay. According to actual measurements: natural water content is 28.7%, wet density is 1.93 g / cm 3 , soil particle density 2.64, porosity 0.790, water saturation 99.0%, liquid limit 27.1%, plasticity index 8.4, direct quick shear cohesion 9.5kPa, internal friction angle 13.7°, compression coefficient of consolidation test 0.360MPa -1 , compression modulus 4.75MPa.
[0061] (2) Medium sand. According to actual measurements, the natural water content is 30.2% and the wet density is 1.89 g / cm 3 , soil particle density 2.66, porosity 1.319, water saturation 90.3%, liquid limit 26.4%, plasticity index 6.1, direct quick shear cohesion 14.8kPa, internal friction angle 7.4°, compression coefficient of consolidation test 0.320MPa -1 , compression modulus 4.95MPa.
[0062] (3) Silty silt. According to actual measurements, the natural water content is 29.2% and the wet density is 1.87 g / cm 3 , soil particle density 2.64, porosity 0.939, water saturation 88.3%, liquid limit 33.9%, plasticity index 12.2, direct quick shear cohesion 13.3kPa, internal friction angle 6.6°, compression coefficient of consolidation test 0.370MPa -1 , compression modulus 4.82MPa.
[0063] (4) Silty clay. According to actual measurements, the natural water content is 49.5% and the wet density is 1.68 g / cm 3 , soil particle density 2.63, porosity 1.276, water saturation 96.1%, liquid limit 40.4%, plasticity index 15.1, direct quick shear cohesion 3.8kPa, internal friction angle 2.3°, compression coefficient of consolidation test 0.977MPa -1 , compression modulus 2.65MPa.
[0064] Separate the sealed soil samples by category, air-dry them, grind them, and pass them through a 5mm sieve for later use.
[0065] In summary: According to the Engineering Geological Survey Report of this bridge, #The detailed drilling hole data, on-site soil layer or soil sample test and inspection of the main pier cap show that: # The silty soft soil layer where the main pier cap is located has the characteristics of "high water content, large porosity, low bearing capacity and low shear strength". The soft soil has high water content, low bearing capacity and poor physical and mechanical properties.
[0066] In this test example, three water-cement ratios of cement slurry of 0.50, 0.60 and 0.70 and three volume ratios of cement to silty soft soil of 1:0.27, 1:0.30 and 1:0.33 are selected to design the components of the silty soft soil reinforcement layer.
[0067] 1. Prepare cement slurry
[0068] (1) Prepare cement slurry with a water-cement ratio of 0.70. Weigh 9.99 kg of cement and 6.99 kg of mixing water, and mix them to make a cement slurry with a water-cement ratio of 0.70 and a volume of 10 L. Test the fluidity of cement slurry according to T0508-2005 Cement slurry fluidity test method (inverted cone method) in the "Testing Procedures for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020). Test the density of cement slurry according to the volumetric flask method.
[0069] (2) Prepare cement slurry with a water-cement ratio of 0.60. Weigh 11.07 kg of cement and 6.64 kg of mixing water, and mix them to make a cement slurry with a water-cement ratio of 0.60 and a volume of 10 L. Test the fluidity of cement slurry according to T0508-2005 Cement slurry fluidity test method (inverted cone method) in the "Test Procedure for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020). Test the density of cement slurry according to the volumetric flask method.
[0070] (3) Prepare cement slurry with a water-cement ratio of 0.50. Weigh 12.15 kg of cement and 6.08 kg of mixing water, and mix them to make a cement slurry with a water-cement ratio of 0.50 and a volume of 10 L. Test the fluidity of cement slurry according to T0508-2005 Cement slurry fluidity test method (inverted cone method) in the "Test Procedure for Cement and Cement Concrete for Highway Engineering" (JTG3420-2020). Test the density of cement slurry according to the volumetric flask method.
[0071] 2. Trial mix of cement silt soft soil
[0072] (1) Prepare the sample. One day before the design and preparation of the components, the air-dried moisture content of the measured silty soft soil was 2.5%, and the predetermined moisture content was 49.5% (simulating the moisture content of the silty silty clay to be reinforced in the construction site project). The amount of water to be added was calculated according to the formula (T 0102-2) in Article 2.2 of the T0102-2007 Soil Sample and Sample Preparation in the "Highway Geotechnical Test Code" (JTG 3430-2020), mixed evenly, and the material was sealed for 1 day to prepare a certain number of silty soft soil samples. After measuring 1m 3 The wet soil mass of silty soft soil is 1690kg / m when the moisture content is 49.5%. 3 ,spare.
[0073] (2) Known conditions. 1m 3 The wet soil mass of silty soft soil when the moisture content is 49.5% is 1690 kg / m 3 The mass of cement required for 10L of cement slurry with a water-cement ratio of 0.50 is 12.15kg, the mass of cement required for 10L of cement slurry with a water-cement ratio of 0.60 is 11.07kg, and the mass of cement required for 10L of cement slurry with a water-cement ratio of 0.70 is 9.99kg.
[0074] (3) Indoor cement silt soft soil. In the test room, according to the selected cement slurry water-cement ratio and the volume ratio of the silt soft soil reinforcement layer, mix the cement silt soft soil of trial mix 1 to trial mix 9 respectively:
[0075] Trial mix 1: The water-cement ratio of cement slurry is 0.70, and the volume ratio of cement to silt soft soil is 1:0.27.
[0076] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3 (270L) The required cement mass in the cement slurry is 270kg and the mixing water mass is 189kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pier construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0077] ① Weigh the masses of various raw materials. The mass of cement is 8.10kg, the mass of mixing water is 5.67kg, and the mass of silty soft soil is 50.70kg.
[0078] ② Preparation method and mixing time. a. Pour the weighed mass of cement into a mortar mixer, add the weighed mass of mixing water and stir for 60 seconds to make cement slurry; b. Pour the weighed mass of silty soft soil into a single-shaft mixer and stir for 60 seconds to disperse the silty soft soil particles, add the prepared cement slurry, and stir for 720 seconds to make cement silty soft soil.
[0079] ③ Specimen preparation. According to the specimen preparation method in Appendix A.2.3 of the Cement-Soil Mix Design Code (JGJ / T 233-2011), cubic specimens with a size of 70.7 mm × 70.7 mm × 70.7 mm were formed, and two groups (each group of specimens consisted of 6 specimens) of unconfined compressive strength specimens were made. One group of specimens was used to measure the 3d unconfined compressive strength, and the other group of specimens was used to measure the 28d unconfined compressive strength.
[0080] ④ Specimen curing. The unconfined compressive strength specimens shall be cured to the age specified in the relevant test in accordance with the specimen curing method in Appendix A.2.4 of the "Cement-Soil Mix Design Code" (JGJ / T 233-2011).
[0081] Trial mix 2: The water-cement ratio of cement slurry is 0.70, and the volume ratio of cement to silt soft soil is 1:0.30.
[0082] According to the above, we can know that every 1m 3 The mass of wet muddy soil required for the muddy soft soil reinforcement layer is 1690kg; 3 (300L) The required cement mass in the cement slurry is 300kg and the mixing water mass is 210kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pedestal construction. The mixing quantity of each plate of cement silt soft soil is 0.03m 3 .
[0083] ① Weigh the masses of various raw materials. The mass of cement is 9.00kg, the mass of mixing water is 6.30kg, and the mass of silty soft soil is 50.70kg.
[0084] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0085] Trial mix three: The water-cement ratio of cement slurry is 0.70, and the volume ratio of cement to silt soft soil is 1:0.33.
[0086] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3(330L) The required cement mass in the cement slurry is 330kg and the mixing water mass is 231kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pedestal construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0087] ① Weigh the masses of various raw materials. The mass of cement is 9.90kg, the mass of mixing water is 6.93kg, and the mass of silty soft soil is 50.70kg.
[0088] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0089] Trial mix 4: The water-cement ratio of cement slurry is 0.60, and the volume ratio of cement to silt soft soil is 1:0.27.
[0090] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3 (270L) The required cement mass in the cement slurry is 299kg and the mixing water mass is 179kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pier construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0091] ① Weigh the masses of various raw materials. The mass of cement is 8.97kg, the mass of mixing water is 5.37kg, and the mass of silty soft soil is 50.70kg.
[0092] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0093] Trial mix 5: The water-cement ratio of cement slurry is 0.60, and the volume ratio of cement to silt soft soil is 1:0.30.
[0094] According to the above, we can know that every 1m 3 The mass of wet muddy soil required for the muddy soft soil reinforcement layer is 1690kg; 3(300L) The required cement mass in the cement slurry is 332kg and the mixing water mass is 199kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pedestal construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0095] ① Weigh the masses of various raw materials. The mass of cement is 9.96kg, the mass of mixing water is 5.97kg, and the mass of silty soft soil is 50.70kg.
[0096] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0097] Trial mix six: The water-cement ratio of cement slurry is 0.60, and the volume ratio of cement to silt soft soil is 1:0.33.
[0098] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3 (330L) The required cement mass in the cement slurry is 365kg and the mixing water mass is 219kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pedestal construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0099] ① Weigh the masses of various raw materials. The mass of cement is 10.95kg, the mass of mixing water is 6.57kg, and the mass of silty soft soil is 50.70kg.
[0100] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0101] Trial mix seven: The water-cement ratio of cement slurry is 0.50, and the volume ratio of cement to silt soft soil is 1:0.27.
[0102] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3(270L) The required cement mass in the cement slurry is 328kg and the mixing water mass is 164kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pier construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0103] ① Weigh the masses of various raw materials. The mass of cement is 9.84kg, the mass of mixing water is 4.92kg, and the mass of silty soft soil is 50.70kg.
[0104] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0105] Trial mix eight: The water-cement ratio of cement slurry is 0.50, and the volume ratio of cement to silt soft soil is 1:0.30.
[0106] According to the above, we can know that every 1m 3 The mass of wet muddy soil required for the muddy soft soil reinforcement layer is 1690kg; 3 (300L) The required cement mass in the cement slurry is 365kg and the mixing water mass is 182kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pier construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0107] ① Weigh the masses of various raw materials. The mass of cement is 10.95kg, the mass of mixing water is 5.46kg, and the mass of silty soft soil is 50.70kg.
[0108] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0109] Trial mix nine: The water-cement ratio of cement slurry is 0.50, and the volume ratio of cement to silt soft soil is 1:0.33.
[0110] According to the above, we can know that every 1m 3 The mass of wet muddy soft soil required for the muddy soft soil reinforcement layer is 1690kg; 3(330L) The required cement mass in the cement slurry is 401kg and the mixing water mass is 201kg. The cement slurry is mixed with a UJZ-15 vertical mortar mixer, and the cement silt soft soil is mixed with a HJW-60 single-horizontal shaft mixer, simulating the mixing method of deep mixers in bridge pedestal construction. The mixing quantity of cement silt soft soil per plate is 0.03m 3 .
[0111] ① Weigh the masses of various raw materials. The mass of cement is 12.03kg, the mass of mixing water is 6.03kg, and the mass of silty soft soil is 50.70kg.
[0112] ② Preparation method, mixing time, specimen preparation and specimen curing. The preparation method, mixing time, specimen preparation and specimen curing are the same as those in Trial Mix 1.
[0113] 3. Cement silt soft soil quality inspection
[0114] For the cement silt soft soil prepared in Trial Mixes 1 to 9, the setting time test was carried out according to the T0592-2020 cement mortar setting time test method in the "Test Code for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020); for the curing specimens of Trial Mixes 1 to 9, the 3d and 28d unconfined compressive strength tests were carried out according to the unconfined compressive strength test method in Appendix B.2 of the "Cement Soil Mix Design Code" (JGJ / T 233-2011). The test results are shown in Table 1.
[0115] Table 1 Cement slurry and cement silt soft soil test results
[0116]
[0117] According to the test results of setting time and 28d unconfined compressive strength of cement slurry and cement muddy soft soil in Table 1, combined with strength and economy, a comprehensive analysis was conducted, and Trial Mix 5 was selected as Comparative Example 1, which is the initial component of cement muddy soft soil indoors, that is, the mass ratio of cement slurry (Comparative Example 1) is cement: mixing water = 332: 199 (unit: kg / m 3 )(water-cement ratio is 0.60); the volume ratio of cement-muddy soft soil is, silty soft soil: cement slurry = 1:0.30.
[0118] On the basis of the indoor initial components (Comparative Example 1), silica fume, nano silicon dioxide, talcum powder and early strength water reducing agent raw materials are added, stirred evenly, and quickly solidified to form a silty soft soil reinforcement layer.
[0119] In the initial component (Comparative Example 1), the amount of mixing water required when the water-cement ratio is 0.60 is 199 kg. The amount of mixing water after adding the early strength water reducer is 179 kg, and the amount of cement is 298 kg. The amount of silica fume is 8% of the amount of cement, and the amount of silica fume is 23.84 kg; the amount of nano-silicon dioxide is 1% of the amount of cement, and the amount of nano-silicon dioxide is 2.98 kg; the amount of talcum powder is 5% of the amount of cement, and the amount of talcum powder is 14.90 kg; the amount of early strength water reducer is 1.5% of the amount of cement, and the amount of early strength water reducer is 4.47 kg.
[0120] The calculated composition (mass ratio) of cement slurry is: cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducer: mixing water = 298: 23.84: 2.98: 14.90: 4.47: 179 (unit: kg / m 3 )(water-cement ratio is 0.60).
[0121] While keeping the quality of mixing water unchanged, the water-cement ratio of cement slurry was increased or decreased by 0.05 (i.e., the water-cement ratio was 0.55, 0.60, and 0.65), and the volume ratios of the silt soft soil reinforcement layer were 1:0.27, 1:0.30, and 1:0.33, respectively. Nine groups of silt soft soil reinforcement layer component designs were carried out.
[0122] Example 1
[0123] The mass ratio of cement slurry is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 325: 26.00: 3.25: 16.25: 4.88: 179 (unit: kg / m 3 )(water-cement ratio is 0.55);
[0124] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.27.
[0125] Example 2
[0126] The mass ratio of cement slurry is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 325: 26.00: 3.25: 16.25: 4.88: 179 (unit: kg / m 3 )(water-cement ratio is 0.55);
[0127] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.30.
[0128] Example 3
[0129] The mass ratio of cement slurry is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 325: 26.00: 3.25: 16.25: 4.88: 179 (unit: kg / m 3 )(water-cement ratio is 0.55);
[0130] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.33.
[0131] Example 4
[0132] The mass ratio of cement slurry is: cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 298: 23.84: 2.98: 14.90: 4.47: 179 (unit: kg / m 3 )(water-cement ratio is 0.60);
[0133] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.27.
[0134] Example 5
[0135] The mass ratio of cement slurry is: cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 298: 23.84: 2.98: 14.90: 4.47: 179 (unit: kg / m 3 )(water-cement ratio is 0.60);
[0136] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.30.
[0137] Example 6
[0138] The mass ratio of cement slurry is: cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 298: 23.84: 2.98: 14.90: 4.47: 179 (unit: kg / m 3 )(water-cement ratio is 0.60);
[0139] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.33.
[0140] Example 7
[0141] The mass ratio of cement paste is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 275: 22.00: 2.75: 13.75: 4.13: 179 (unit: kg / m 3 )(water-cement ratio is 0.65);
[0142] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.27.
[0143] Example 8
[0144] The mass ratio of cement paste is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 275: 22.00: 2.75: 13.75: 4.13: 179 (unit: kg / m 3 )(water-cement ratio is 0.65);
[0145] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.30.
[0146] Example 9
[0147] The mass ratio of cement paste is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 275: 22.00: 2.75: 13.75: 4.13: 179 (unit: kg / m 3 )(water-cement ratio is 0.65);
[0148] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.33.
[0149] In the laboratory, a UJZ-15 vertical mortar mixer was used to mix cement slurry, and an HJW-60 single-horizontal shaft mixer was used to mix cement silt soft soil, simulating the mixing method of deep mixers mixing silt soft soil in bridge cap construction. The volume ratio of the silt soft soil reinforcement layer is silt soft soil: cement slurry = 1:0.27 (i.e., 1m 3 Or 1000L of silty soft soil as the basis, 0.27m 3 or 270L cement slurry); the volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.30 (i.e., 1m 3 Or 1000L of silty soft soil as the base, 0.30m 3 or 300L cement slurry); the volume ratio of the muddy soft soil reinforcement layer is muddy soft soil: cement slurry = 1:0.33 (i.e., 1m 3 Or 1000L of silty soft soil as the base, 0.33m 3 or 330L cement slurry); and 1m 3 The mass of wet soil of silty soft soil is 1690kg. The mixing quantity of each plate of silty soft soil reinforcement layer is 0.03m 3 The quality of various raw materials is as follows:
[0150] Example 1: Cement mass is 325kg / m 3 ×0.27×0.03m 3 =2.633kg, the mass of silica fume is 26.00kg / m3 ×0.27×0.03m 3 =0.211kg, the mass of nano-silicon dioxide is 3.25kg / m 3 ×0.27×0.03m 3 =0.026kg, the mass of talcum powder is 16.25kg / m 3 ×0.27×0.03m 3 =0.132kg, the mass of early strength water reducing agent is 4.88kg / m 3 ×0.27×0.03m 3 =0.040kg, the mass of mixing water is 179kg / m 3 ×0.27×0.03m 3 =1.450kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0151] Example 2: Cement mass is 325kg / m 3 ×0.30×0.03m 3 =2.925kg, silica fume mass is 26.00kg / m 3 ×0.30×0.03m 3 =0.234kg, the mass of nano-silicon dioxide is 3.25kg / m 3 ×0.30×0.03m 3 =0.029kg, the mass of talcum powder is 16.25kg / m 3 ×0.30×0.03m 3 =0.146kg, the mass of early strength water reducing agent is 4.88kg / m 3 ×0.30×0.03m 3 =0.044kg, the mass of mixing water is 179kg / m 3 ×0.30×0.03m 3 =1.611kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0152] Example 3: Cement mass is 325kg / m 3 ×0.33×0.03m 3 =3.218kg, silica fume mass is 26.00kg / m 3 ×0.33×0.03m 3 =0.257kg, the mass of nano-silicon dioxide is 3.25kg / m 3 ×0.33×0.03m3 =0.032kg, the mass of talcum powder is 16.25kg / m 3 ×0.33×0.03m 3 =0.161kg, the mass of early strength water reducing agent is 4.88kg / m 3 ×0.33×0.03m 3 =0.048kg, the mass of mixing water is 179kg / m 3 ×0.33×0.03m 3 =1.772kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0153] Example 4: Cement mass is 298kg / m 3 ×0.27×0.03m 3 =2.414kg, the mass of silica fume is 23.84kg / m 3 ×0.27×0.03m 3 =0.193kg, the mass of nano-silicon dioxide is 2.98kg / m 3 ×0.27×0.03m 3 =0.024kg, the mass of talcum powder is 14.90kg / m 3 ×0.27×0.03m 3 =0.121kg, the mass of early strength water reducing agent is 4.47kg / m 3 ×0.27×0.03m 3 =0.036kg, the mass of mixing water is 179kg / m 3 ×0.27×0.03m 3 =1.450kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0154] Example 5: Cement mass is 298kg / m 3 ×0.30×0.03m 3 =2.682kg, the mass of silica fume is 23.84kg / m 3 ×0.30×0.03m 3 =0.215kg, the mass of nano-silicon dioxide is 2.98kg / m 3 ×0.30×0.03m 3 =0.027kg, the mass of talcum powder is 14.90kg / m 3 ×0.30×0.03m 3=0.134kg, the mass of early strength water reducing agent is 4.47kg / m 3 ×0.30×0.03m 3 =0.040kg, the mass of mixing water is 179kg / m 3 ×0.30×0.03m 3 =1.611kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0155] Example 6: Cement mass is 298kg / m 3 ×0.33×0.03m 3 =2.950kg, the mass of silica fume is 23.84kg / m 3 ×0.33×0.03m 3 =0.236kg, the mass of nano-silicon dioxide is 2.98kg / m 3 ×0.33×0.03m 3 =0.030kg, the mass of talcum powder is 14.90kg / m 3 ×0.33×0.03m 3 =0.148kg, the mass of early strength water reducing agent is 4.47kg / m 3 ×0.33×0.03m 3 =0.044kg, the mass of mixing water is 179kg / m 3 ×0.33×0.03m 3 =1.772kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0156] Example 7: Cement mass is 275kg / m 3 ×0.27×0.03m 3 =2.228kg, the mass of silica fume is 22.00kg / m 3 ×0.27×0.03m 3 =0.178kg, the mass of nano-silicon dioxide is 2.75kg / m 3 ×0.27×0.03m 3 =0.022kg, the mass of talcum powder is 13.75kg / m 3 ×0.27×0.03m 3 =0.111kg, the mass of early strength water reducing agent is 4.13kg / m 3 ×0.27×0.03m 3 =0.033kg, the mass of mixing water is 179kg / m3 ×0.27×0.03m 3 =1.450kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0157] Example 8: Cement mass is 275kg / m 3 ×0.30×0.03m 3 =2.475kg, silica fume mass is 22.00kg / m 3 ×0.30×0.03m 3 =0.198kg, the mass of nano-silicon dioxide is 2.75kg / m 3 ×0.30×0.03m 3 =0.025kg, the mass of talcum powder is 13.75kg / m 3 ×0.30×0.03m 3 =0.124kg, the mass of early strength water reducing agent is 4.13kg / m 3 ×0.30×0.03m 3 =0.037kg, the mass of mixing water is 179kg / m 3 ×0.30×0.03m 3 =1.611kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3 =50.700kg.
[0158] Example 9: Cement mass is 275 kg / m 3 ×0.33×0.03m 3 =2.723kg, silica fume mass is 22.00kg / m 3 ×0.33×0.03m 3 =0.218kg, the mass of nano-silicon dioxide is 2.75kg / m 3 ×0.33×0.03m 3 =0.027kg, the mass of talcum powder is 13.75kg / m 3 ×0.33×0.03m 3 =0.136kg, the mass of early strength water reducing agent is 4.13kg / m 3 ×0.33×0.03m 3 =0.041kg, the mass of mixing water is 179kg / m 3 ×0.33×0.03m 3 =1.772kg, the mass of silty soft soil is 1690kg / m 3 ×0.03m 3=50.700kg.
[0159] The preparation methods and stirring times of Examples 1 to 9 are as follows:
[0160] a. Weigh the raw materials according to the above raw material mass, pour the weighed mass of cement, silica fume, nano-silicon dioxide, talcum powder, and early strength water reducing agent into the mortar mixer and stir for 60 seconds to mix the powder evenly, add the weighed mass of mixing water and stir for 120 seconds to make cement slurry.
[0161] b. Pour the weighed silt soft soil into a single-horizontal shaft mixer and stir for 60 seconds to disperse the silt soft soil particles. Add the prepared cement slurry and stir for 720 seconds to prepare the silt soft soil reinforcement layer mixture.
[0162] Preparation of specimens for Examples 1 to 9: According to the specimen preparation method in Appendix A.2.3 of the "Code for Design of Cement-Soil Mix Ratio" (JGJ / T 233-2011), cubic specimens with a molding size of 70.7 mm×70.7 mm×70.7 mm were made, and 2 groups (each group of specimens consisted of 6 specimens) of unconfined compressive strength specimens were made, one group of specimens was used to measure the 3d unconfined compressive strength, and the other group of specimens was used to measure the 28d unconfined compressive strength.
[0163] Curing of the specimens of Examples 1 to 9: Curing to the age specified in the relevant test in accordance with Appendix A.2.4 of the Standard Specification for Cement-Soil Mix Ratio Design (JGJ / T 233-2011).
[0164] The cement slurries prepared in Examples 1 to 9 were tested for fluidity according to T0508-2005 Cement Paste Fluidity Test Method (Inverted Cone Method) in the Standard "Testing Procedures for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020). Density was tested according to the volumetric flask method.
[0165] The silty soft soil reinforcement layer mixture prepared in Examples 1 to 9 was tested for setting time according to the T0592-2020 cement mortar setting time test method in the "Test Code for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020); the curing specimens of Examples 1 to 9 were tested for 3d and 28d unconfined compressive strength according to the unconfined compressive strength test method in Appendix B.2 of the "Cement Soil Mix Design Code" (JGJ / T233-2011). The test results are shown in Table 2.
[0166] Table 2 Test results of cement slurry and silty soft soil reinforcement layer mixture
[0167]
[0168] According to the test results of setting time, 3d and 28d unconfined compressive strength of cement slurry and muddy soft soil reinforcement layer mixture in Table 2, a comprehensive analysis was conducted from the perspectives of strength and economy, and three kinds of indoor design components of muddy soft soil reinforcement layer of Example 1, Example 5 and Example 9 were selected for construction verification on the construction site. That is:
[0169] Construction verification component 1 (Example 1)
[0170] The mass ratio of cement slurry is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 325: 26.00: 3.25: 16.25: 4.88: 179 (unit: kg / m 3 )(water-cement ratio is 0.55);
[0171] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.27.
[0172] Construction verification component 2 (Example 5)
[0173] The mass ratio of cement slurry is: cement: silica fume: nano-silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 298: 23.84: 2.98: 14.90: 4.47: 179 (unit: kg / m 3 )(water-cement ratio is 0.60);
[0174] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.30.
[0175] Construction verification component 3 (Example 9)
[0176] The mass ratio of cement paste is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 275: 22.00: 2.75: 13.75: 4.13: 179 (unit: kg / m 3 )(water-cement ratio is 0.65);
[0177] The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.33.
[0178] This application has been verified in the construction of the foundation pit of the 7# main pier cap of a bridge in the Guangdong Delta Plain. A cement slurry mixing station and a storage tank are set up near the silty soft soil layer that needs to be reinforced at the construction site of the 7# main pier cap of the bridge. After the cement slurry is mixed, the cement slurry is pumped into the grouting pipe of the deep mixer by the slurry hose. The three indoor design components of the silty soft soil reinforcement layer of the proposed embodiment 1, embodiment 5, and embodiment 9 are respectively verified by deep mixing construction of three cylindrical piles.
[0179] On the bridge 7 # During the construction of the main pier foundation, the silty soft soil reinforcement layer was formed by the cylindrical pile deep mixer mixing method. The specific forming method is as follows:
[0180] 1. Spraying and sinking: Connect the slurry hose to the storage tank, mortar pump and deep mixer, turn on the deep mixer motor, and the mixer blades turn in opposite directions. With the help of the deep mixer equipment's deadweight, the drill rod sinks vertically at a uniform speed of 0.3-0.5m / min to the designed reinforcement depth. While sinking, spray and stir at a uniform speed of 0.3-0.5m / min. When the drill rod enters 0.5m from the top of the silty soil layer, turn on the mortar pump, and press the cement slurry from the central tube of the deep mixer into the silty soil layer at a grouting pressure of 0.40MPa-0.60MPa. The cement slurry and the silty soil layer are mixed by the mixer blades, and the slurry is sprayed while mixing until the designed reinforcement depth. During the spraying process, the cement slurry is continuously stirred. During the spraying construction, a slurry flow meter is used to control the slurry delivery speed, and the outlet pressure of the grouting pump is maintained at 0.40MPa-0.60MPa, and the slurry delivery speed must be kept constant. During shotcrete spraying, an automatic shotcrete recorder must be used to record: shotcrete volume, drill lifting speed and bored pile length indicators.
[0181] 2. Spraying and lifting: When the deep mixer sinks to the designed reinforcement depth, after mixing and spraying at the end of the cylindrical pile for 30 seconds, it is stirred and lifted at a uniform speed of 0.3-0.5m / min, and the cement slurry is sprayed at a grouting pressure of 0.40MPa-0.60MPa. The cement slurry is continuously pressed into the silty soil layer from the central tube of the deep mixer. The cement slurry and the silty soil layer are mixed by the mixing blades of the mixer. The slurry is sprayed while stirring until it is 0.5m away from the top surface of the silty soil layer. Stop spraying and the mixing process is completed.
[0182] 3. Re-mixing: During implementation, each cylindrical pile must repeat the previous operation of four mixing and four spraying. The first sinking mixing and lifting mixing are both at a speed of 0.3 or 0.4m / min; during re-mixing, the sinking mixing is at a speed of 0.4 or 0.5m / min, and the lifting mixing is at a speed of 0.3 or 0.4m / min, and there is a short pause between the two mixing. The normal forming time of each cylindrical pile is not less than 40min, and the spraying pressure is not less than 0.4MPa. The re-spraying and re-mixing method is conducive to making up for the insufficient amount of spraying in one time and accelerating the slurry reaction process.
[0183] 4. Shift: After mixing a cylindrical pile, the next cylindrical pile should be constructed in the same way. Repeat the above steps. After reinforcement is completed every day, use clean water to clean the storage tank, mortar pump, deep mixer and corresponding pipelines for reuse.
[0184] Preparation of cement slurry and forming construction of silty soft soil reinforcement layer:
[0185] 1. Cement Slurry Preparation
[0186] According to the volume ratio of one cylindrical pile and the volume ratio of the silty soft soil reinforcement layer, calculate the amount of cement slurry required for mixing one cylindrical pile. Design the cement slurry preparation method and mixing time according to the indoor components of the silty soft soil reinforcement layer. Mix cement, silica fume, nano-silicon dioxide, talcum powder, early strength water reducer, and mixing water according to the component ratio of construction verification component 1 to construction verification component 3 to prepare cement slurries with different components. For cement slurry, the fluidity test method of cement slurry T0508-2005 (inverted cone method) in the "Test Procedure for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020) is used to test the fluidity of cement slurry. Test the density of cement slurry according to the volumetric flask method.
[0187] 2. Construction of the reinforcement layer of silty soft soil
[0188] (1) At a location where a cylindrical pile is required to reinforce a silty soft soil layer, a cylindrical pile is formed according to the above-mentioned silty soft soil reinforcement layer forming method.
[0189] (2) For each construction verification component, three cylindrical piles need to be formed according to the above-mentioned method for forming the silty soft soil reinforcement layer. For the above-mentioned construction verification components 1 to 3, a total of nine cylindrical piles need to be formed.
[0190] (3) After each cylindrical pile is formed, it shall be naturally cured until the age of 28 days, and the pile number and construction verification component shall be marked and recorded. During the curing period of the cylindrical pile, the foundation pit shall not be excavated to disturb the cylindrical pile.
[0191] After the 9 cylindrical piles were naturally cured to 28 days old, core samples with a diameter of 84 mm were drilled. Core samples were cut from the top, middle and bottom of each cylindrical pile and processed into a group of unconfined compressive strength test pieces. According to the unconfined compressive strength test method in Appendix B.2 of the "Cement-Soil Mix Design Code" (JGJ / T 233-2011), the unconfined compressive strength test was carried out, and the core sample evaluation of the cylindrical pile molding integrity was carried out. The test results of cement slurry and silty soft soil reinforcement layer are shown in Table 3.
[0192] Table 3 Test results of cement slurry and silty soft soil reinforcement layer
[0193]
[0194]
[0195] The test results of cement slurry and silt soft soil reinforcement layer show that:
[0196] 1. Construction Verification Comparison of test results of component 1 and embodiment 1:
[0197] 1) The difference between the cement slurry density and the cement slurry density is 0.02g / cm 3 Less than 0.03g / cm 3 The parallel test allowable error requirements. The cement slurry fluidity difference between the two is 0.3s and is almost consistent. The 3d unconfined compressive strength of 1.14MPa in Example 1 is greater than the 3d design strength requirement of 0.8MPa, and the 28d unconfined compressive strength of 1.61MPa is greater than the 28d design strength requirement of 1.0MPa. Among the 28d unconfined compressive strengths of the three cylindrical piles in construction verification component 1, the minimum value is 1.54MPa, the maximum value is 1.62MPa, and the average value is 1.58MPa. The minimum value deviates from the average value by 0.04MPa, and the maximum value deviates from the average value by 0.04MPa. Its average strength of 1.58MPa is greater than the 28d design strength requirement of 1.0MPa.
[0198] 2) Construction Verification The test results of Component 1 and Example 1 both meet the requirements of relevant standards and specifications.
[0199] 2. Construction Verification Comparison of test results of component 2 and embodiment 5:
[0200] 1) The difference between the cement slurry density and the cement slurry density is 0.01g / cm 3 Less than 0.03g / cm 3 The parallel test allowable error requirements. The cement slurry fluidity difference between the two is 0.3s and is almost consistent. The 3d unconfined compressive strength of 1.07MPa in Example 5 is greater than the 3d design strength requirement of 0.8MPa, and the 28d unconfined compressive strength of 1.51MPa is greater than the 28d design strength requirement of 1.0MPa. Among the 28d unconfined compressive strengths of the three cylindrical piles in construction verification component 2, the minimum value is 1.45MPa, the maximum value is 1.53MPa, and the average value is 1.49MPa. The minimum value deviates from the average value by 0.04MPa, and the maximum value deviates from the average value by 0.04MPa. Its average strength of 1.49MPa is greater than the 28d design strength requirement of 1.0MPa.
[0201] 2) Construction Verification The test results of Component 2 and Example 5 both meet the requirements of relevant standards and specifications.
[0202] 3. Construction Verification Comparison of test results of component 3 and embodiment 9:
[0203] 1) The difference between the cement slurry density and the cement slurry density is 0.02g / cm 3 Less than 0.03g / cm 3The parallel test allowable error requirements. The cement slurry fluidity difference between the two is 0.2s and is close to the same. The 3d unconfined compressive strength of 1.04MPa in Example 9 is greater than the 3d design strength requirement of 0.8MPa, and the 28d unconfined compressive strength of 1.47MPa is greater than the 28d design strength requirement of 1.0MPa. Among the 28d unconfined compressive strengths of the three cylindrical piles in the construction verification component 3, the minimum value is 1.43MPa, the maximum value is 1.49MPa, and the average value is 1.46MPa. The minimum value deviates from the average value by 0.03MPa, and the maximum value deviates from the average value by 0.03MPa. Its average strength of 1.46MPa is greater than the 28d design strength requirement of 1.0MPa.
[0204] 2) Construction Verification The test results of Component 3 and Example 9 both meet the requirements of relevant standards and specifications.
[0205] 4. From Comparative Example 1 and Examples 1, 5, 9 and Construction Verification Components 1-3, it can be seen that the cement slurry of the present invention obtained by adding silica fume, nano-silicon dioxide, talcum powder and early strength water reducing agent to the cement slurry (cement and mixing water) in Comparative Example 1 has the following effects: (1) The cement usage is saved by 7 to 57 kg / m 3 (2) The cement slurry density increased by 0.03-0.16 g / cm 3 (3) The fluidity of cement slurry decreased by 3.2 to 6.5 seconds. (4) The initial setting time was shortened by 12 to 27 minutes, and the final setting time was shortened by 17 to 25 minutes. (5) The 3d unconfined compressive strength increased by 0.57 to 0.67 MPa, and the 28d unconfined compressive strength increased by 0.32 to 0.47 MPa.
[0206] 5. Evaluation of cylindrical pile core samples of construction verification components 1 to 3:
[0207] 1) Evaluation of the three cylindrical pile core samples of construction verification component 1: the core samples are continuous, complete, hard, evenly mixed, columnar, and well consolidated overall.
[0208] 2) Evaluation of the three cylindrical pile core samples of construction verification component 2: the core samples are continuous, complete, hard, evenly mixed, columnar, and well consolidated overall.
[0209] 3) Evaluation of the three cylindrical pile core samples of construction verification component 3: the core samples are basically complete, hard, basically evenly mixed, columnar, partially blocky, and generally consolidated overall.
[0210] The construction verification component 2 (Example 5) of the silty soft soil reinforcement layer that has been verified on the construction site and meets the strength, core sample evaluation and economic rationality is used as the construction control basis for the silty soft soil reinforcement layer of the 7# main pier cap of the bridge project.
[0211] According to the Technical Specifications for Highway Bridge and Culvert Construction (JTG / T3650-2020), the allowable quality deviation of the quantity of ingredients for concrete mixing in "centralized mixing stations" is stipulated: the allowable measurement deviation of cement, dry admixtures, mixing water, and admixtures is ±1%.
[0212] The design components of the silty soft soil reinforcement layer are determined as follows:
[0213] The preferred mass ratio of cement slurry is: cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water = 296-300: 23.61-24.06: 2.96-3.00: 14.76-15.04: 4.43-4.51: 178-180 (unit: kg / m 3 ) The volume ratio of the silty soft soil reinforcement layer is silty soft soil: cement slurry = 1:0.28-0.30. (It should be noted that the volume ratio of the silty soft soil reinforcement layer is based on the volume of the silty soft soil as a constant of 1, a fixed value; the volume of cement slurry is a variable value).
[0214] The present invention adopts silty soft soil as the reference material of the silty soft soil reinforcement layer to construct the skeleton structure of the silty soft soil reinforcement layer; sprays and presses cement slurry prepared by cement, silica fume, nano-silicon dioxide, talcum powder, early strength water-reducing agent and mixing water into the silty soft soil; stirs, squeezes and fills the pores between the silty soft soil particles with a deep mixer, and quickly solidifies to form the silty soft soil reinforcement layer. The technical problems of the silty soft soil layer being difficult to form, high permeability, poor water-stopping performance, low strength, low bearing capacity, small lateral supporting force, poor foundation pit stability and pollution of river water quality during construction can be solved, and the following can be achieved: saving cement consumption and reducing the construction cost of the silty soft soil reinforcement layer; reducing the moisture content and water saturation of each stratum of the silty soft soil; improving the silty soft soil reinforcement The uniformity and overall consolidation of the layer; reduce the porosity of the silty soft soil layer, improve the impermeability and water-stopping performance of the silty soft soil reinforcement layer, prevent the construction sewage in the foundation pit of the cap from infiltrating into the nearby river outside the foundation pit through the pores between the stratum soil particles, polluting the river water quality, or the groundwater outside the foundation pit of the cap from infiltrating into the foundation pit through the pores between the stratum soil particles, causing water accumulation in the foundation pit, seriously affecting the construction of the 7# main pier cap; make the 3d unconfined compressive strength of the silty soft soil reinforcement layer reach the design requirement of the 28d unconfined compressive strength (i.e. ≥1.0MPa), quickly improve the bearing capacity and lateral support force of the silty soft soil reinforcement layer, effectively shorten the maintenance age of the silty soft soil reinforcement layer, excavate the cap pit in advance, shorten the construction period of the cap, and reduce the construction cost; improve the technical effect of the stability of the cap pit. The design components of the silt soft soil reinforcement layer of the present application, in addition to being used in deep foundation pit support projects near water excavation to improve the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer, can also be used according to the purpose of the engineering construction, using the same cement slurry components, by adjusting the mass ratio of the various components of the cement slurry and the volume ratio of silt soft soil to cement slurry. It can be applied to silt soft soil reinforcement construction in geotechnical engineering fields such as industrial and civil building foundations, road subgrades, river embankments and seepage prevention and protection, and deep foundation pit excavation and protection of urban rail transit, so as to achieve the same effect of improving the strength, bearing capacity, lateral support and water-stopping performance of the silt soft soil reinforcement layer.
[0215] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A silty soft soil reinforcement layer for supporting deep foundation pits near water. It is characterized in that The reinforcement layer includes a reference material and cement slurry; the reference material is silty soft soil, and the cement slurry includes cement, silica fume, nano silicon dioxide, talcum powder, early strength water reducing agent and mixing water; the mass ratio of cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 275-325: 22-26: 2.75-3.25: 13.75-16.25: 4.13-4.88: 178-180; The silty soft soil and cement slurry are mixed in a volume ratio of 1:0.27-0.
33.
2. The silty soft soil reinforcement layer for supporting deep foundation pits excavated near water according to claim 1, It is characterized in that The reference material is silty soft soil prepared by mixing silty clay, medium sand, silty silt sand and silty silty clay in a blending ratio of 10%:11%:9%:70% of the stratum thickness.
3. The silty soft soil reinforcement layer for supporting deep foundation pits excavated near water according to claim 1, It is characterized in that The reference material and cement slurry are mixed in a volume ratio of 1:0.28-0.
30.
4. The silty soft soil reinforcement layer for supporting deep foundation pits excavated near water according to claim 1, It is characterized in that The mass ratio of cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 296-300: 23.61-24.06: 2.96-3.00: 14.76-15.04: 4.43-4.51: 178-180.
5. The silty soft soil reinforcement layer for supporting deep foundation pits excavated near water according to claim 4, It is characterized in that The mass ratio of cement: silica fume: nano silicon dioxide: talcum powder: early strength water reducing agent: mixing water in the cement slurry is 298:23.84:2.98:14.90:4.47:
179.
6. The silty soft soil reinforcement layer for supporting deep foundation pits excavated near water according to claim 1, It is characterized in that The silty soft soil is sieved through a 5 mm sieve.
7. A construction method for forming a silty soft soil reinforcement layer for supporting deep foundation pits near water. It is characterized in that The following steps are involved: S1: Connect the slurry hose to the storage tank, mortar pump and deep mixer, start the deep mixer, and use the deep mixer's deadweight to vertically sink the drill rod at a uniform speed of 0.3-0.5m / min to the designed reinforcement depth. While sinking, spray and stir at a uniform speed of 0.3-0.5m / min. When the drill rod is 0.5m away from the top of the silty soil layer, start the mortar pump and continuously press the cement slurry from the central tube of the deep mixer into the silty soil layer. The mixer's stirring blades stir the cement slurry with the silty soil layer, and spray while stirring until the designed reinforcement depth is reached. S2: After the deep mixer sinks to the designed reinforcement depth and mixes and sprays at the end of the cylindrical pile, it is mixed and lifted at a uniform speed of 0.3-0.5m / min, and cement slurry is sprayed at the same time. The cement slurry is continuously pressed into the silty soil layer from the central tube of the deep mixer. The cement slurry and the silty soil layer are mixed by the mixing blades of the mixer. The slurry is sprayed while mixing until it is 0.5m away from the top surface of the silty soil layer. The spraying is stopped, and the mixing process is completed once; S3: Each cylindrical pile must be re-mixed to obtain a reinforced layer formed cylindrical pile.
8. The method for forming a silty soft soil reinforcement layer for supporting a deep foundation pit near water according to claim 7, It is characterized in that The grouting pressure of the cement slurry is 0.40MPa to 0.60MPa.
9. The method for forming a silty soft soil reinforcement layer for supporting a deep foundation pit near water excavation according to claim 7, It is characterized in that In step S3, each cylindrical pile is subjected to four-stirring and four-spraying stirring, and the first sinking stirring and lifting stirring are both carried out at a speed of 0.3 or 0.4 m / min; during the repeated stirring, the sinking stirring is carried out at a speed of 0.4 or 0.5 m / min, and the lifting stirring is carried out at a speed of 0.3 or 0.4 m / min, and a short pause is made between the two stirrings.
10. The method for forming a silty soft soil reinforcement layer for supporting a deep foundation pit near water according to claim 7 or 8, It is characterized in that In step S3, the normal forming time of each cylindrical pile is not less than 40 minutes, and the shotcrete pressure is not less than 0.4 MPa.
Citation Information
Cited By
Novel ecological base material for ecological restoration of river bank side slope as well as preparation method and application of novel ecological base material
CN119822740A