Tailing curing early strength filling material as well as preparation and use methods thereof
By preparing a tailings solidification early-strength backfill material, the problem of reduced strength in the later stage of the backfill body was solved, achieving the effect of high early strength and stable later strength. It is suitable for underground backfilling in mines and protects the safety of surface buildings.
Patent Information
- Application Number
- CN202411166927.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
In existing technologies, the backfill material using ordinary silicate cement to solidify tailings suffers from reduced strength and insufficient durability in the later stages, making it difficult to effectively control ground pressure and protect surface structures.
Tailings solidification early-strength filling material is used, which includes industrial solid waste, crystal nucleus materials, low-temperature calcined early-strength composite materials and other materials. Through mixing and grinding, a mixed powder with a high specific surface area is formed, and a filling material with high early strength and stable later strength is prepared.
It improves the consolidation of tailings, achieves high early strength, stable growth in later strength, good durability, and low cost, and is suitable for underground filling materials in both metal and non-metal mines.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mine filling materials, and in particular to a tailings solidification early strength filling material and a preparation and use method thereof. Background Art
[0002] With the increase of mining depth and the increasing complexity of mining conditions, ground pressure control and safety issues are becoming increasingly prominent. Therefore, it is necessary to use filling materials to manage ground pressure, control surrounding rock collapse and surface subsidence, protect surface buildings, and ease large-area ground pressure activities to protect the safety of underground working space.
[0003] The backfill mining method commonly used at present is a mining method that gradually fills the goaf with backfill materials as the mining face advances. During backfilling, cement and other cementitious materials and tailings are prepared into slurry-like cementitious materials, which are transported to the mining site by pipelines through hydraulic or mechanical means. After the slurry-like cementitious materials solidify, they form a solidified body with a certain strength and stable volume, thereby filling the goaf.
[0004] However, when backfill mining is carried out by solidifying sulfur-containing tailings using ordinary Portland cement as a cementitious material, the strength of the backfill body decreases in the later stage and the durability cannot be guaranteed. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a tailings solidification early strength filling material and a preparation and use method thereof.
[0006] To solve the above problems, the technical solution adopted by the present invention is: In the first aspect, a tailings solidification early strength filling material is provided, which comprises the following components by weight: 20 to 90 parts of industrial solid waste, 4 to 30 parts of crystal nucleus materials, 5 to 25 parts of other materials, 1 to 15 parts of low-temperature calcined early strength composite materials, 0.05 to 1 parts of grinding aids, 0.1 to 3 parts of active stimulants, 0.1 to 2 parts of suspending agents, 0.05 to 2 parts of pumping agents and 0.2 to 3 parts of reinforcing agents.
[0007] As an embodiment of the invention, the industrial solid waste is selected from any one of water-quenched ferromanganese slag, water-quenched ferrochromium slag, water-quenched ferromagnesium slag, air-quenched blast furnace slag, water-quenched blast furnace slag, and water-quenched vanadium-titanium slag, or a mixture of any two or more thereof.
[0008] As an embodiment of the invention, the crystal nucleus material is selected from any one of steel slag, silicate cement, ordinary silicate cement, silicate cement clinker, aluminate cement, and aluminate cement clinker, or a mixture of any two or more thereof.
[0009] As an embodiment of the invention, the other materials are selected from any one of basalt, alunite, phosphogypsum, copper gypsum, natural gypsum, and salt gypsum, or a mixture of any two or more of them.
[0010] As an embodiment of the invention, the preparation method of the low-temperature calcined early-strength composite material is as follows: ①, according to the dry weight percentage, take 10-50 parts of coal gangue with a particle size of 0.01-1 cm, 25-35 parts of titanium gypsum, 10-20 parts of red mud, 10-20 parts of carbide slag, 5-10 parts of magnesite with a particle size of 0.01-1 cm, and 5-10 parts of lithium slag and grind them together to a specific surface area of 350-380m 2 / kg of mixed powder; ②, the mixed powder obtained in step ① is calcined at 500-800°C for 30-60min, and then the calcined mixed powder is ventilated and rapidly cooled by a fan so that the temperature is reduced to 70-80°C at a rate of 150-250°C / min to obtain the low-temperature calcined early-strength composite material.
[0011] As an embodiment of the invention, the grinding aid is selected from any one of diethylene glycol, calcium stearate, coal, isopropyl alcohol, propylene glycol, diethanolamine, sodium polyphosphate, or a mixture of any two or more thereof; The active stimulant is selected from any one of potassium sulfate, zinc sulfate, potassium alum, aluminum sulfate, calcined dolomite, and sodium silicate, or a mixture of any two or more thereof; The suspending agent is selected from any one of xanthan gum, redispersible latex powder, glue, dextrin, latex powder, carboxymethyl cellulose or a mixture of any two or more thereof; The pumping agent is selected from any one of calcium citrate, calcium gluconate, magnesium lignin sulfonate, calcium lignin sulfonate, sodium lignin sulfonate, and borax, or a mixture of any two or more thereof; The reinforcing agent is selected from any one of calcium formate, lithium carbonate, aluminum oxide, zinc oxide, potassium formate, sodium formate, and lithium chloride, or a mixture of any two or more thereof.
[0012] In a second aspect, a method for preparing a tailings-solidified early-strength filling material as described in the first aspect is provided, which comprises step S1: Step S1: Grind industrial solid waste, crystal nucleus material, other materials, low-temperature calcined early strength composite material, and grinding aid to a specific surface area of 450-510 m 2 / kg, and then mixed and ground with active stimulants, suspending agents, pumping agents and enhancers until the specific surface area is 545~655m 2 / kg, specifically 547~651m 2 / kg, the tailings solidified early strength filling material is obtained.
[0013] In a third aspect, a method for preparing a tailings-cured early-strength filling material as described in the first aspect is provided, which comprises step S2: Step S2: Grind the industrial solid waste, crystal nucleus material, other materials, low-temperature calcined early-strength composite material, grinding aid, active stimulant, suspending agent, pumping agent and reinforcing agent together until the specific surface area is 545-655m 2 / kg, specifically 547~651m 2 / kg, the tailings solidified early strength filling material is obtained.
[0014] In a fourth aspect, a method for using the tailings solidified early strength filling material as described in the first aspect is provided, the method comprising: By weight, 1 part of tailings solidification early strength filling material, 3 to 80 parts of mine tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry with a weight concentration of (45 to 85)%, which is transported to the filling site through a pipeline system by gravity or pumping to fill the goaf.
[0015] As an embodiment of the invention, the mine dressing tailings are selected from any one of metal mine tailings, graded tailings, overflow tailings, waste rock, non-metallic mine tailings, and machine-made sand, or a mixture of any two or more thereof.
[0016] The beneficial effects of adopting the above technical solution are: (1) The present invention grinds coal gangue with a particle size of 0.01 to 1 cm, titanium gypsum, 10 to 20 parts of red mud, carbide slag, magnesite with a particle size of 0.01 to 1 cm, and lithium slag to a particle size of 350 to 380 m 2 / kg, calcined at low temperature (500-800℃) and rapidly cooled to obtain a low-temperature calcined early-strength composite material, which has the advantages of simple preparation method, low cost and wide application range.
[0017] (2) The present invention can obtain tailings solidification early strength filling material by mixing industrial solid waste, crystal nuclei, other materials, low-temperature calcined early strength composite material, grinding aid, active stimulant, suspending agent, pumping agent and reinforcing agent. The tailings solidification early strength filling material has the characteristics of wide source of raw materials, low cost, harmlessness, non-toxicity and pollution-free; it not only makes rational use of solid waste, but also reduces pollution to the environment.
[0018] (3) The tailings solidification early strength filling material provided by the present invention can improve the consolidation amount with tailings while meeting the requirements of early strength and late strength, and can achieve a maximum of 1 part of tailings solidification early strength filling material consolidating 80 parts of tailings.
[0019] (4) The tailings solidification early strength filling material provided by the present invention has the advantages of high early strength, stable growth of late strength, good durability, etc. The preparation method is simple, the cost is low, and it is easy to industrialize production. It can be widely used as underground filling material for metal and non-metal mines. DETAILED DESCRIPTION
[0020] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.
[0021] Example 1 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 30 parts of coal gangue with a particle size of 0.1 cm, 31 parts of titanium gypsum, 16 parts of red mud, 14 parts of calcium carbide slag, 8 parts of magnesite with a particle size of 0.1 cm, and 9 parts of lithium slag together to a specific surface area of 367m 2 / kg of mixed powder; ②, after the mixed powder obtained in step ① is calcined at 500°C for 60 min, it is rapidly cooled by ventilation with a fan so that the temperature is reduced to 80°C at a rate of 150°C / min to obtain low-temperature calcined early-strength composite material I.
[0022] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 20 parts of water-quenched vanadium-titanium slag, crystal nucleus material: 25 parts of steel slag, 5 parts of aluminate cement, other materials: 25 parts of basalt, 15 parts of low-temperature calcined early strength composite material I, grinding aid: 0.4 parts of diethylene glycol, 0.6 parts of sodium polyphosphate were first ground to a specific surface area of 452m 2 / kg; then, grind it with the active stimulant: 3 parts of potassium sulfate, suspending agent: 2 parts of xanthan gum, pumping agent: 2 parts of calcium citrate, and enhancer: 3 parts of calcium formate until the specific surface area is 597m 2 / kg, and the tailings solidified early strength filling material I is obtained.
[0023] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidification early strength filling material I, 3 parts of metal mine whole tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry I with a weight concentration of 60%.
[0024] The material mechanical properties test of the hardened body of filling slurry I was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:1.5. The specific strength test results are shown in Table 1.
[0025] Table 1 Example 2 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 10 parts of coal gangue with a particle size of 0.5 cm, 35 parts of titanium gypsum, 20 parts of red mud, 20 parts of carbide slag, 10 parts of magnesite with a particle size of 0.5 cm, and 10 parts of lithium slag together to a specific surface area of 356m 2 / kg of mixed powder; ②. After the mixed powder obtained in step ① is calcined at 700°C for 40 min, it is rapidly cooled by ventilation with a fan so that the temperature is reduced to 75°C at a rate of 210°C / min to obtain low-temperature calcined early-strength composite material II.
[0026] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 35 parts of water-quenched ferromanganese slag, crystal nucleus material: 25 parts of silicate cement, other materials: 22 parts of alum stone, 13 parts of low-temperature calcined early strength composite material II, and 0.7 parts of grinding aid: calcium stearate were first ground to a specific surface area of 479m 2 / kg, and then grind it with active stimulant: 2 parts of zinc sulfate, suspending agent: 0.9 parts of redispersible latex powder, 0.7 parts of dextrin, pumping agent: 0.05 parts of calcium gluconate, and reinforcing agent: 2.7 parts of lithium carbonate until the specific surface area is 651m 2 / kg, and the tailings solidified early strength filling material II is obtained.
[0027] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidification early strength filling material II, 8 parts of metal mine graded tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry II with a weight concentration of 70%.
[0028] The material mechanical properties test of the hardened body of filling slurry II was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:4. The specific strength test results are shown in Table 2.
[0029] Table 2 Example 3 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 45 parts of coal gangue with a particle size of 1 cm, 27 parts of titanium gypsum, 14 parts of red mud, 12 parts of calcium carbide slag, 6 parts of magnesite with a particle size of 0.8 cm, and 5 parts of lithium slag together to a specific surface area of 372m 2 / kg of mixed powder; ②. After the mixed powder obtained in step ① is calcined at 500°C for 55 min, it is rapidly cooled by ventilation with a fan so that the temperature is reduced to 78°C at a rate of 160°C / min to obtain low-temperature calcined early-strength composite material III.
[0030] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 45 parts of water-quenched chromite slag, crystal nucleus material: 20 parts of ordinary Portland cement, other materials: 18 parts of phosphogypsum, 11 parts of low-temperature calcined early strength composite material III, and 0.5 parts of grinding aid: coal were first ground to a specific surface area of 508m 2 / kg; then, it was mixed and ground with active stimulant: 2 parts of potassium alum, 0.5 parts of calcined dolomite, suspending agent: 1.3 parts of bone glue, pumping agent: 1.5 parts of magnesium lignin sulfonate, and reinforcing agent: 2.2 parts of alumina until the specific surface area was 553m 2 / kg, and the tailings solidified early strength filling material III is obtained.
[0031] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidification early strength filling material III, 16 parts of metal mine overflow tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry III with a weight concentration of 45%.
[0032] The material mechanical properties test of the hardened body of filling slurry III was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:8. The specific strength test results are shown in Table 3.
[0033] Table 3 Example 4 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 20 parts of coal gangue with a particle size of 0.01 cm, 33 parts of titanium gypsum, 18 parts of red mud, 18 parts of calcium carbide slag, 9 parts of magnesite with a particle size of 0.05 cm, and 8 parts of lithium slag together to a specific surface area of 361m 2 / kg of mixed powder; ②, after the mixed powder obtained in step ① is calcined at 550°C for 45 min, it is rapidly cooled by ventilation with a blower so that the temperature is reduced to 70°C at a rate of 250°C / min to obtain a low-temperature calcined early-strength composite material IV.
[0034] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 60 parts of water-quenched magnesia iron slag, crystal nucleus material: 15 parts of silicate cement clinker, other materials: 9 parts of copper gypsum, 6 parts of salt gypsum, 8 parts of low-temperature calcined early strength composite material IV, grinding aid: 0.3 parts of isopropanol, 1.5 parts of active stimulant: aluminum sulfate, 0.1 parts of dextrin, 1 part of pumping agent: 1 part of calcium lignin sulfonate, 0.6 parts of reinforcing agent: zinc oxide, 1 part of sodium formate were mixed and ground together to a specific surface area of 649m 2 / kg, and the tailings solidified early strength filling material IV is obtained.
[0035] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidification early strength filling material IV, 20 parts of metal mine waste rock and appropriate amount of water are stirred and mixed to form a mixed filling slurry IV with a weight concentration of 75%. The metal mine waste rock is lead-zinc mine waste rock, and its particle size ranges from 0.01 to 8 mm, and the particle size less than 80 mesh accounts for 35%.
[0036] The material mechanical properties test of the hardened body of filling slurry III was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:10. The specific strength test results are shown in Table 4.
[0037] Table 4 Example 5 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 50 parts of coal gangue with a particle size of 0.1 cm, 25 parts of titanium gypsum, 12 parts of red mud, 10 parts of calcium carbide slag, 5 parts of magnesite with a particle size of 0.01 cm, and 7 parts of lithium slag together to a specific surface area of 352m 2 / kg of mixed powder; ②, after the mixed powder obtained in step ① is calcined at 650°C for 50 min, it is rapidly cooled by ventilation with a fan so that the temperature is reduced to 75°C at a rate of 200°C / min to obtain a low-temperature calcined early-strength composite material V.
[0038] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 75 parts of water-quenched blast furnace slag, crystal nucleus material: 10 parts of aluminate cement, other materials: 10 parts of natural gypsum, 4 parts of low-temperature calcined early strength composite material V, grinding aid: 0.1 parts of propylene glycol, 1 part of active stimulant: calcined dolomite, 1 part of suspending agent: latex powder, 0.5 parts of pumping agent: sodium lignin sulfonate, 1 part of reinforcing agent: potassium formate, are mixed and ground together to a specific surface area of 547 m 2 / kg, and the tailings solidified early strength filling material V is obtained.
[0039] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidification early strength filling material V, 30 parts of non-metallic mine tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry V with a weight concentration of 80%.
[0040] The material mechanical properties test of the hardened body of filling slurry III was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:15. The specific strength test results are shown in Table 5.
[0041] Table 5 Example 6 1. Preparation of low-temperature calcined early-strength composite materials ①, according to the dry weight percentage, mix and grind 40 parts of coal gangue with a particle size of 0.5 cm, 29 parts of titanium gypsum, 10 parts of red mud, 16 parts of calcium carbide slag, 7 parts of magnesite with a particle size of 0.9 cm, and 6 parts of lithium slag together to a specific surface area of 379m 2 / kg of mixed powder; ②, after the mixed powder obtained in step ① is calcined at 800°C for 30 min, it is rapidly cooled by ventilation with a fan so that the temperature is reduced to 78°C at a rate of 250°C / min to obtain a low-temperature calcined early-strength composite material VI.
[0042] 2. Preparation of tailings solidification early strength filling materials By weight, industrial solid waste: 30 parts of water-quenched ferromanganese slag, 60 parts of air-quenched blast furnace slag, crystal nucleus material: 4 parts of aluminate cement clinker, other materials: 5 parts of salt gypsum, 1 part of low-temperature calcined early strength composite material VI, grinding aid: 0.05 parts of diethanolamine, 0.1 parts of active stimulant: sodium silicate, 0.5 parts of suspending agent: carboxymethyl cellulose, 1.1 parts of pumping agent: borax, 0.6 parts of calcium gluconate, and 0.2 parts of reinforcing agent: lithium chloride are mixed and ground together to a specific surface area of 599m 2 / kg, and the tailings solidified early strength filling material VI is obtained.
[0043] 3. Prepare mixed filling slurry By weight, 1 part of tailings solidified early strength filling material VI, 80 parts of machine-made sand and an appropriate amount of water are stirred and mixed to form a mixed filling slurry VI with a weight concentration of 85%.
[0044] The material mechanical properties test of the hardened body of filling slurry III was carried out in accordance with the group standard T / CECS 10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions using PO42.5 cement-lime-sand ratio of 1:40. The specific strength test results are shown in Table 6.
[0045] Table 6 Comparative Example 1 The preparation method of this comparative example is the same as that of Example 2, except that step 1 of preparing the low-temperature calcined early-strength composite material is omitted, and step 2 of preparing the low-temperature calcined early-strength composite material is omitted.
[0046] Comparative Example 2 The preparation method of this comparative example is the same as that of Example 2, except that industrial solid waste is omitted in step 2.
[0047] Comparative Example 3 The preparation method of this comparative example is the same as that of Example 2, except that the crystal nucleus material is omitted in step 2.
[0048] Comparative Example 4 The preparation method of this comparative example is the same as that of Example 2, except that other materials are omitted in step 2.
[0049] Comparative Example 5 The preparation method of this comparative example is the same as that of Example 2, except that: in step 2, the final mixing and grinding is performed to a specific surface area of 492 m 2 / kg.
[0050] Comparative Example 6 The preparation method of this comparative example is the same as that of Example 2, except that: in step ② of step 1, the mixed powder obtained in step ① is calcined at 1000°C for 40 min, and then rapidly cooled by ventilation with a fan to reduce the temperature to 75°C at a rate of 200°C / min to obtain the material.
[0051] Effect example: The material mechanical properties test of the mixed filling slurry hardened body obtained in Comparative Examples 1 to 6 was carried out in accordance with the group standard T / CECS10091-2020 "Tailings Filling Glue Solids", and a comparative test was carried out under the same conditions as Example 2. The specific strength test comparison is shown in Table 7.
[0052] Table 7 It can be seen from the strength data in Tables 1 to 6 that, under the same test conditions, when the proportion of tailings solidified early strength filling material is twice the proportion of cement solidified tailings, the strength at all ages is higher than the strength of cement. This is due to the mutual coordination between the various materials that make up the tailings solidified early strength filling material, which improves the early strength of the tailings solidified early strength filling material and makes the later strength increase steadily.
[0053] The data in Table 7 are the strength data of comparative examples. Comparative Example 1 omits the low-temperature calcined early-strength composite material from step 1 and step 2 in Example 2; Comparative Example 2 omits the industrial solid waste from step 2 in Example 2; Comparative Example 3 omits the crystal nucleus material from step 2 in Example 2; Comparative Example 4 omits other materials from step 2 in Example 2; Comparative Example 5 finally grinds the composite material from step 2 in Example 2 to a specific surface area of 492 m 2 / kg.
[0054] After the ratio of Example 2 was changed in Comparative Examples 1-5, the strength data of Comparative Examples 1-5 in Table 7 show that the strength at each age is reduced. This is because the change in the material ratio of the tailings solidification early strength filling material makes it impossible for the materials constituting the tailings solidification early strength filling material to fully coordinate with each other, resulting in low strength at each age.
[0055] The preparation method of comparative example 6 is the same as that of example 2, except that: in step 2 of step 1, the mixed powder obtained in step 1 is calcined at 1000°C for 55 minutes, and then rapidly cooled by ventilation to obtain a low-temperature calcined early-strength composite material. From the strength data of comparative example 6 in Table 7, it can be seen that the strength at 7 days and 14 days increases slightly, and the strength at 28 days decreases slightly. Although the strength is not greatly affected, the temperature is increased and the production cost increases.
[0056] The tailings solidification early strength filling material of the present invention has the advantages of high early strength, stable growth of late strength, good durability, etc., and the preparation method is simple, the cost is low, and it is easy to industrialize production, and can be widely used as underground filling materials for metal and non-metal mines. The superior performance of the tailings solidification early strength filling material of the present invention is verified by comparing the performance tests of the embodiment with the comparative example.
Claims
1. A tailings solidified early strength filling material, characterized in that: The invention comprises the following components by weight: 20-90 parts of industrial solid waste, 4-30 parts of crystal nucleus materials, 5-25 parts of other materials, 1-15 parts of low-temperature calcined early-strength composite materials, 0.05-1 parts of grinding aids, 0.1-3 parts of active stimulants, 0.1-2 parts of suspending agents, 0.05-2 parts of pumping agents and 0.2-3 parts of reinforcing agents.
2. The tailings solidified early strength filling material according to claim 1, characterized in that: The industrial solid waste is selected from any one of water-quenched ferromanganese slag, water-quenched ferrochromium slag, water-quenched ferromagnesium slag, air-quenched blast furnace slag, water-quenched blast furnace slag, and water-quenched vanadium-titanium slag, or a mixture of any two or more thereof.
3. The tailings solidified early strength filling material according to claim 1, characterized in that: The crystal nucleus material is selected from any one of steel slag, Portland cement, ordinary Portland cement, Portland cement clinker, aluminate cement, and aluminate cement clinker, or a mixture of any two or more thereof.
4. The tailings solidified early strength filling material according to claim 1, characterized in that: The other materials are selected from any one of basalt, alunite, phosphogypsum, copper gypsum, natural gypsum, and salt gypsum, or a mixture of any two or more of them.
5. The tailings solidified early strength filling material according to claim 1, characterized in that: The preparation method of the low-temperature calcined early-strength composite material is as follows: ①, according to dry weight, take 10-50 parts of coal gangue with a particle size of 0.01-1 cm, 25-35 parts of titanium gypsum, 10-20 parts of red mud, 10-20 parts of carbide slag, 5-10 parts of magnesite with a particle size of 0.01-1 cm, and 5-10 parts of lithium slag and grind them together until the specific surface area is 350-380m 2 / kg of mixed powder; ②, the mixed powder obtained in step ① is calcined at 500-800°C for 30-60min, and then the calcined mixed powder is ventilated and rapidly cooled by a fan so that the temperature is reduced to 70-80°C at a rate of 150-250°C / min to obtain the low-temperature calcined early-strength composite material.
6. The tailings solidified early strength filling material according to claim 1, characterized in that: The grinding aid is selected from any one of diethylene glycol, calcium stearate, coal, isopropyl alcohol, propylene glycol, diethanolamine, and sodium polyphosphate, or a mixture of any two or more thereof; The active stimulant is selected from any one of potassium sulfate, zinc sulfate, potassium alum, aluminum sulfate, calcined dolomite, and sodium silicate, or a mixture of any two or more thereof; The suspending agent is selected from any one of xanthan gum, redispersible latex powder, glue, dextrin, latex powder, carboxymethyl cellulose or a mixture of any two or more thereof; The pumping agent is selected from any one of calcium citrate, calcium gluconate, magnesium lignin sulfonate, calcium lignin sulfonate, sodium lignin sulfonate, and borax, or a mixture of any two or more thereof; The enhancer is selected from any one of calcium formate, lithium carbonate, aluminum oxide, zinc oxide, potassium formate, sodium formate, and lithium chloride, or a mixture of any two or more thereof.
7. A method for preparing a tailings solidified early strength filling material according to any one of claims 1 to 6, characterized in that: It includes step S1: Step S1: Grind industrial solid waste, crystal nucleus material, other materials, low-temperature calcined early strength composite material, and grinding aid to a specific surface area of 450-510 m 2 / kg, and then grind it together with the active stimulant, suspending agent, pumping agent and enhancer until the specific surface area is 545~655m 2 / kg, and the tailings solidified early strength filling material is obtained.
8. A method for preparing a tailings solidified early strength filling material according to any one of claims 1 to 6, characterized in that: It includes step S2: Step S2: Grind together industrial solid waste, crystal nucleus material, other materials, low-temperature calcined early-strength composite material, grinding aid, active stimulant, suspending agent, pumping agent, and reinforcing agent until the specific surface area is 545-655 m 2 / kg, and the tailings solidified early strength filling material is obtained.
9. A method for using the tailings solidified early strength filling material according to any one of claims 1 to 6, characterized in that: The method comprises: By weight, 1 part of tailings solidification early strength filling material, 3 to 80 parts of mine beneficiation tailings and an appropriate amount of water are stirred and mixed to form a mixed filling slurry with a weight concentration of (45 to 85)%, which is transported to the filling site through the pipeline system by gravity or pumping to be used for filling the goaf.
10. A method for using the tailings solidified early strength filling material according to claim 9, characterized in that: The mine dressing tailings are selected from any one of metal mine full tailings, graded tailings, overflow tailings, waste rock, non-metallic mine tailings, and machine-made sand, or a mixture of any two or more of them.
Citation Information
Cited By
Damp and hot nanometer crystal nucleus early strength agent, tailing solidification filling material and preparation method and application of damp and hot nanometer crystal nucleus early strength agent and tailing solidification filling material
CN121135219A