Recycling processing formula of stone waste residue powder

By adding nanomaterials and shape memory wires to the reuse processing formula of stone waste residue powder, a composite gelling system is formed, which solves the problem of insufficient mechanical properties and durability of stone waste residue in the construction field, and significantly improves the strength and density of the mortar , achieving improvement in project quality.

CN119019144APending Publication Date: 2024-11-26吴志金
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924365.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Stone waste slag faces insufficient mechanical properties and durability in the reuse of construction fields, and the prior art is difficult to effectively improve its physical and chemical properties, while taking into account cost and process feasibility.

Method used

A stone waste residue powder reuse processing formula, including silicate cement, fly ash, styrene butadiene latex powder, lime, stone waste residue powder, river sand, sesap stone powder, modified filler, hydroxypropyl methylcellulose Ether and water reducing agent form a composite gelling system through synergistic effects, improving the early and late strength of the mortar, and improving mechanical properties through nanomaterials and shape memory wires.

Benefits of technology

It significantly improves the comprehensive performance of the mortar, enhances its early and later strength, improves the microstructure, reduces porosity, improves density and compressive strength, and reduces water consumption, delays the cement hydration process, ensuring Project quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a stone waste residue powder recycling processing formula. The stone waste residue powder recycling processing formula comprises the following components in parts by mass: 5-10 parts of Portland cement, 1-6 parts of fly ash, 2-7 parts of styrene-butadiene latex powder, 1-5 parts of lime, 12-17 parts of stone waste residue powder, 50-60 parts of river sand, 1-3 parts of sepiolite powder, 3-7 parts of modified filler, 0.01-0.03 part of hydroxypropyl methyl cellulose ether, 0.01-0.03 part of a water reducing agent and 22-27 parts of water. The mortar prepared by utilizing the processing formula has good constructability, and is beneficial to improving the construction efficiency and ensuring the engineering quality. The stone waste residue powder used in the invention has a high specific surface area, so the contact area between the stone waste residue powder and a cement hydration product is increased, the hydration reaction of cement is promoted, and the strength of the mortar is improved. Meanwhile, the fineness of the stone waste residue powder is beneficial to improving the microstructure of the mortar, reducing the porosity and improving the compactness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a formula for recycling and processing stone waste slag powder. Background Art

[0002] Stone waste is a by-product generated during stone mining and processing, including scraps, dust, fragments and stones that do not meet size or quality standards. If these wastes are not treated, they will not only waste resources, but also pollute the environment, occupy land and may pose safety hazards. However, there are many ways to reuse stone waste, which can turn waste into treasure.

[0003] Although the reuse of stone waste in the construction field has opened up new ways for resource conservation and environmental protection, it still faces many challenges at the technical level. Improving the physical and chemical properties of stone waste is a technical challenge. Since the original stone waste has a gap in mechanical properties and durability compared with natural stone or specially produced building materials, how to improve its performance through physical or chemical methods becomes a key issue. For example, improving its structural density through mechanical compaction or heat treatment, or changing its chemical composition by adding chemical additives, thereby improving the stability and strength of the waste as a building material. Research in this area needs to focus not only on performance improvement, but also on cost and process feasibility to ensure the economic benefits of the technology. Summary of the invention

[0004] The purpose of the present invention is to provide a stone waste slag powder recycling processing formula, the mortar prepared by the formula has good construction performance, helps to improve construction efficiency and ensure project quality.

[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a stone waste slag powder recycling processing formula, comprising the following components in parts by weight: 5-10 parts of silicate cement, 1-6 parts of fly ash, 2-7 parts of styrene-butadiene latex powder, 1-5 parts of lime, 12-17 parts of stone waste slag powder, 50-60 parts of river sand, 1-3 parts of sepiolite powder, 3-7 parts of modified filler, 0.01-0.03 parts of hydroxypropyl methylcellulose ether, 0.01-0.03 parts of water reducer, and 22-27 parts of water.

[0006] Furthermore, the preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:6-8:0.05-0.08, an ethanol aqueous solution with a volume fraction of 70-80%, and a silane coupling agent KH550, react at 60-70° C. for 7-10 hours, filter and dry to obtain a modified mixed powder; (2) Mix 1 part by mass of porous rubber powder and 0.2-0.3 parts by mass of modified mixed powder, and then add 0.2-0.4 parts by mass of shape memory metal wire. Stir evenly at 160-180°C, then heat to 300-320°C, stir for 20-30 minutes, cool to room temperature, and crush to obtain a modified filler.

[0007] Furthermore, the mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.2-0.5:1.3-1.7.

[0008] Furthermore, the porosity of the modified filler is 13-16%, and the particle size distribution is 10-40 μm.

[0009] Furthermore, the shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0010] Furthermore, the viscosity of the hydroxypropyl methylcellulose ether is 90,000 to 110,000 mPa·s.

[0011] Furthermore, the stone waste powder is quartz artificial stone waste, with a specific surface area of ​​100-500m 2 / kg, apparent density is 1600~2000kg / m 3 , loose bulk density is 650~850kg / m 3 The loose porosity is 55~70%, and the compact density is 700~900kg / m 3 The tight porosity is 40~60% and the SiO2 content is greater than 85%.

[0012] Furthermore, the water reducer is a polycarboxylic acid water reducer with a solid content of 25-34% and a water reduction rate of 34%-38%.

[0013] Furthermore, raw materials are weighed according to the formula, stirred and mixed evenly to obtain mortar.

[0014] Compared with the prior art, the advantages and beneficial effects of the present invention are: 1. The present invention selects a variety of raw materials, and through the effect of synergistic enhancement, the proportion of each component in the formula is carefully designed, so that various materials can work synergistically to jointly improve the comprehensive performance of the mortar, form a composite cementitious system, and improve the early and late strength of the mortar.

[0015] 2. The stone waste powder used in the present invention has a high specific surface area, which increases the contact area with the cement hydration product, promotes the hydration reaction of the cement, and thus improves the strength of the mortar. At the same time, the fineness of the stone waste powder helps to improve the microstructure of the mortar, reduce the porosity, and improve the density.

[0016] 3. The nanomaterials in the modified filler can significantly improve the mechanical properties of the mortar by adding shape memory wires. Nanomaterials can fill the microcracks inside the mortar to form a denser structure; shape memory wires can return to their original shape when heated, which helps to relieve internal stress during the hardening process of the mortar, prevent cracking, and further enhance the compressive strength of the mortar. At the same time, styrene-butadiene latex powder is a polymer powder that can form a continuous film in the mortar, enhance the flexibility and adhesion of the mortar, and improve crack resistance. Hydroxypropyl methylcellulose ether, as a water retaining agent, can effectively retain moisture in the mortar, delay the cement hydration process, ensure that the cement is fully hydrated, and thus improve the strength and water retention of the mortar. Polycarboxylic acid water reducer can significantly reduce the water consumption of the mortar at a low dosage without sacrificing or even improving the working performance of the mortar. The advantage of this is that it reduces the free water in the mortar, reduces the porosity, and improves the density and strength of the mortar. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Example 1 The present embodiment provides a processing formula for recycling stone waste slag powder, including the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 15 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 5 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0019] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0020] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0021] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0022] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0023] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0024] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0025] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0026] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0027] Example 2 The present embodiment provides a processing formula for recycling stone waste slag powder, including the following components in parts by mass: 5 parts of silicate cement, 1 part of fly ash, 2 parts of styrene-butadiene latex powder, 1 part of lime, 12 parts of stone waste slag powder, 50 parts of river sand, 1 part of sepiolite powder, 3 parts of modified filler, 0.01 part of hydroxypropyl methylcellulose ether, 0.01 part of water reducer, and 22 parts of water.

[0028] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:6:0.05, an ethanol aqueous solution with a volume fraction of 70%, and a silane coupling agent KH550, react at 60° C. for 7 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.2 parts by mass of modified mixed powder were mixed evenly, and 0.2 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 160°C, and then heated to 300°C, stirred for 20 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0029] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.2:1.3.

[0030] The porosity of the modified filler is 16%, and the particle size distribution is 10-40 μm.

[0031] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0032] The viscosity of the hydroxypropyl methylcellulose ether is 90,000 mPa·s.

[0033] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​100m 2 / kg, the apparent density is 1600kg / m 3 , loose bulk density is 650kg / m 3 The loose porosity is 55% and the compact density is 700kg / m 3 , the tight porosity is 40% and the SiO2 content is 86%.

[0034] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 25% and a water reducing rate of 34%.

[0035] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0036] Example 3 The present embodiment provides a processing formula for recycling stone waste slag powder, including the following components in parts by mass: 10 parts of silicate cement, 6 parts of fly ash, 7 parts of styrene-butadiene latex powder, 5 parts of lime, 17 parts of stone waste slag powder, 60 parts of river sand, 3 parts of sepiolite powder, 7 parts of modified filler, 0.03 parts of hydroxypropyl methylcellulose ether, 0.03 parts of water reducer, and 27 parts of water.

[0037] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:8:0.08, an ethanol aqueous solution with a volume fraction of 80%, and a silane coupling agent KH550, react at 70° C. for 10 h, filter and dry, and obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.3 part by mass of modified mixed powder were mixed evenly, and 0.4 part by mass of shape memory metal wire was added. The mixture was stirred evenly at 180°C, and then the temperature was raised to 320°C, stirred for 30 min, cooled to room temperature, and crushed to obtain a modified filler.

[0038] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.5:1.7.

[0039] The porosity of the modified filler is 16%, and the particle size distribution is 10-40 μm.

[0040] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0041] The viscosity of the hydroxypropyl methylcellulose ether is 110,000 mPa·s.

[0042] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​500m 2 / kg, the apparent density is 2000kg / m 3 , loose bulk density is 850kg / m 3 The loose porosity is 70% and the compact density is 900kg / m 3 , the tight porosity is 60% and the SiO2 content is greater than 90%.

[0043] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 34% and a water reducing rate of 38%.

[0044] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0045] Comparative Example 1 The difference between this comparative example and Example 1 is that the mass fractions are different.

[0046] A processing formula for recycling stone waste slag powder includes the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 10 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 10 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0047] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0048] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0049] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0050] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0051] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0052] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0053] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0054] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0055] Comparative Example 2 The difference between this comparative example and Example 1 is that the number of raw materials is different.

[0056] A stone waste powder recycling processing formula includes the following components in parts by mass: 8 parts of silicate cement, 8 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 10 parts of stone waste powder, 55 parts of river sand, 2 parts of sepiolite powder, 5 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0057] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0058] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0059] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0060] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0061] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0062] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0063] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0064] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0065] Comparative Example 3 The difference between this comparative example and Example 1 is that the mass fractions are different.

[0066] A processing formula for recycling stone waste slag powder includes the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 19 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 1 part of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0067] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0068] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0069] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0070] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0071] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0072] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0073] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0074] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0075] Comparative Example 4 The difference between this comparative example and Example 1 is that the mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:1:1.

[0076] A processing formula for recycling stone waste slag powder includes the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 15 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 5 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0077] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0078] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:1:1.

[0079] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0080] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0081] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0082] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0083] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0084] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0085] Comparative Example 5 The difference between this comparative example and Example 1 is that the stone waste slag powder is different.

[0086] A processing formula for recycling stone waste slag powder includes the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 15 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 5 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0087] The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550, react at 65° C. for 8 h, filter and dry to obtain a modified mixed powder; (2) 1 part by mass of porous rubber powder and 0.25 parts by mass of modified mixed powder were mixed evenly, and 0.3 parts by mass of shape memory metal wire was added. The mixture was stirred evenly at 170°C, and then the temperature was raised to 310°C, stirred for 25 minutes, cooled to room temperature, and crushed to obtain a modified filler.

[0088] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0089] The porosity of the modified filler is 14%, and the particle size distribution is 10-40 μm.

[0090] The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

[0091] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0092] The stone waste slag powder is quartz artificial stone waste slag with a specific surface area of ​​80m 2 / kg, the apparent density is 1300kg / m 3 , loose bulk density is 500kg / m 3 The loose porosity is 85% and the compact density is 550kg / m 3 , the tight porosity is 30% and the SiO2 content is 80%.

[0093] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0094] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0095] Comparative Example 6 The difference between this comparative example and Example 1 is that the filler modification method is different.

[0096] A processing formula for recycling stone waste slag powder includes the following components in parts by mass: 8 parts of silicate cement, 3 parts of fly ash, 4 parts of styrene-butadiene latex powder, 3 parts of lime, 15 parts of stone waste slag powder, 55 parts of river sand, 2 parts of sepiolite powder, 5 parts of modified filler, 0.02 parts of hydroxypropyl methylcellulose ether, 0.02 parts of water reducer, and 25 parts of water.

[0097] The preparation method of the modified filler is as follows: nano silicon dioxide, nano calcium carbonate and nano silicon carbide are mixed to obtain a mixed powder, the mixed powder with a mass ratio of 1:7:0.06, an ethanol aqueous solution with a volume fraction of 75%, and a silane coupling agent KH550 are mixed, reacted at 65° C. for 8 hours, filtered and dried to obtain the modified filler.

[0098] The mass ratio of nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide is 1:0.4:1.5.

[0099] The viscosity of the hydroxypropyl methylcellulose ether is 100,000 mPa·s.

[0100] The stone waste powder is quartz artificial stone waste, with a specific surface area of ​​300m 2 / kg, the apparent density is 1800kg / m 3 , loose bulk density is 700kg / m 3 The loose porosity is 65% and the compact density is 800kg / m 3 , the tight porosity is 50% and the SiO2 content is 89%.

[0101] The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 30% and a water reducing rate of 36%.

[0102] Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.

[0103] Performance Testing The properties of the mortars prepared according to the formulas of Examples 1-3 and Comparative Examples 1-6 were measured. The results are shown in Table 1.

[0104] Table 1 Performance test results It can be seen from the above performance test results that the formulas of Examples 1-2 have good effects, especially the comprehensive performance of Example 1 is the most outstanding. However, since the comparative example does not adopt the necessary technical solution, it is obviously worse than the example in the corresponding performance test. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effect.

[0105] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A stone waste slag powder recycling processing formula, characterized in that: The invention comprises the following components in parts by weight: 5-10 parts of silicate cement, 1-6 parts of fly ash, 2-7 parts of styrene-butadiene latex powder, 1-5 parts of lime, 12-17 parts of stone waste slag powder, 50-60 parts of river sand, 1-3 parts of sepiolite powder, 3-7 parts of modified filler, 0.01-0.03 parts of hydroxypropyl methylcellulose ether, 0.01-0.03 parts of water reducing agent and 22-27 parts of water.

2. The stone waste slag powder recycling processing formula according to claim 1 is characterized in that: The preparation method of the modified filler is: (1) Mix nano-silicon dioxide, nano-calcium carbonate and nano-silicon carbide to obtain a mixed powder, mix the mixed powder in a mass ratio of 1:6-8:0.05-0.08, an ethanol aqueous solution with a volume fraction of 70-80%, and a silane coupling agent KH550, react at 60-70° C. for 7-10 hours, filter and dry to obtain a modified mixed powder; (2) Mix 1 part by mass of porous rubber powder and 0.2-0.3 parts by mass of modified mixed powder, and then add 0.2-0.4 parts by mass of shape memory metal wire. Stir evenly at 160-180°C, then heat to 300-320°C, stir for 20-30 minutes, cool to room temperature, and crush to obtain a modified filler.

3. The stone waste slag powder recycling processing formula according to claim 2 is characterized in that: The mass ratio of nano silicon dioxide, nano calcium carbonate and nano silicon carbide is 1:0.2-0.5:1.3-1.

7.

4. The stone waste slag powder recycling processing formula according to claim 2 is characterized in that: The porosity of the modified filler is 13-16%, and the particle size distribution is 10-40 μm.

5. The stone waste slag powder recycling processing formula according to claim 2 is characterized in that: The shape memory metal wire is a titanium-nickel alloy with a diameter of 100-200 microns and a length of 0.3-0.7 mm.

6. The stone waste slag powder recycling processing formula according to claim 1, characterized in that: The viscosity of the hydroxypropyl methylcellulose ether is 90,000 to 110,000 mPa·s.

7. The stone waste slag powder recycling processing formula according to claim 1 is characterized in that: The stone waste slag powder is quartz artificial stone waste slag, and the specific surface area is 100~500m 2 / kg, apparent density is 1600~2000kg / m 3 , loose bulk density is 650~850kg / m 3 The loose porosity is 55~70%, and the compact density is 700~900kg / m 3 The tight porosity is 40~60% and the SiO2 content is greater than 85%.

8. The stone waste slag powder recycling processing formula according to claim 1, characterized in that: The water reducer is a polycarboxylic acid water reducer with a solid content of 25-34% and a water reduction rate of 34%-38%.

9. The stone waste slag powder recycling processing formula according to claim 1, characterized in that: The cement is P.II42.5 cement.

10. The stone waste slag powder recycling processing formula according to claim 1, characterized in that: Weigh the raw materials according to the formula, stir and mix them evenly to obtain mortar.