Fire clay for masonry of magnesia carbon bricks at movable bottom of converter

By using fire mud composed of magnesium sand powder and resin between magnesium carbon bricks for masonry, the loosening and brick extraction problems caused by expansion or shrinkage of magnesium carbon bricks are solved, and the firm combination and safe use of magnesium carbon bricks are achieved. Extend the service life of the converter bottom.

CN119019155APending Publication Date: 2024-11-26JINAN LUDONG REFRACTORY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411131620.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Magnesium carbon bricks loosen, brick extraction, peeling, etc. due to expansion or contraction at different temperatures, which affects the safety and life of the converter smelting process.

Method used

Masonry with fire mud containing magnesium sand powder and resin. By adjusting the thermosetting of the resin and the mass ratio of the thermoplastic resin and the particle size of the magnesium sand powder, a layered structure is formed to stabilize the bond between magnesium carbon bricks and ensure the fire mud. Stability and fluidity at different temperatures avoid the problems of foaming and curing too quickly.

Benefits of technology

It effectively prevents loosening and brick extraction accidents of magnesium carbon bricks, extends the service life of the converter furnace bottom, and improves the safety of the smelting process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides fire clay for masonry of magnesia carbon bricks at the bottom of a converter, and belongs to the technical field of masonry construction of converter lining refractory materials. The fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not larger than 0.5 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.2-5. The appropriate magnesia particle size is selected, so that the stable thickness can be kept during fire clay smearing, and the thermal expansion coefficient of the magnesia carbon brick is absorbed; the two resins are matched for use, so that the problem of heated foaming caused by independent use of thermoplastic resin and the problem of influence on masonry due to high curing speed caused by independent use of thermosetting resin are solved. The furnace bottom magnesia carbon bricks are carbonized by heated resin to form a carbon chain structure in the converter steelmaking process by adopting fire clay masonry, so that expansion of the magnesia carbon bricks is absorbed, the furnace bottom magnesia carbon bricks form a firmly combined whole, accidents such as loosening and brick drawing of the furnace bottom magnesia carbon bricks are prevented, safe use of the converter bottom is guaranteed, and the service life of the converter bottom is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of converter lining refractory material masonry construction, in particular to fire mud for converter live bottom magnesia carbon brick masonry. Background Art

[0002] At present, the new intelligent steelmaking technology of bottom oxygen blowing and bottom powder spraying introduced by large converters has a rapid erosion of the bottom refractory of the converter. The bottom refractory needs to be replaced many times during the entire converter smelting service to synchronize the life of the refractory in other parts. The magnesia carbon bricks of the bottom refractory are generally dry-laid, which causes the magnesia carbon bricks to expand and peel off due to heat; or during the period between steel tapping and steel adding, the magnesia carbon bricks refractory shrink in volume due to the lower furnace temperature, which may cause the bottom bricks to fall off during the shaking process of the converter smelting operation, resulting in accidents such as steel penetration and leakage at the bottom. Summary of the invention

[0003] The technical problem to be solved by the present invention is: how to alleviate the loosening, brick pulling, peeling and other phenomena of magnesia carbon bricks caused by expansion or contraction at different temperatures by using specific fire clay for masonry.

[0004] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0005] The invention discloses fire clay for laying magnesia-carbon bricks for active bottom of converter. The fire clay contains magnesia powder and resin. The particle size of the magnesia powder is ≤0.5 mm. The resin contains thermosetting resin and thermoplastic resin. The mass ratio of thermosetting resin to thermoplastic resin in the resin is 0.2-5.

[0006] Preferably, the fire mud is maintained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 0.5 to 5 mm.

[0007] Preferably, the particle size of the magnesia powder is ≤0.3 mm.

[0008] Preferably, the fire mud is maintained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 3 to 5 mm.

[0009] Preferably, the particle size of the magnesia powder is ≤0.2 mm.

[0010] Preferably, the fire mud is maintained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 0.5 to 3 mm.

[0011] Preferably, when the season is summer, the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.2-2.

[0012] Preferably, when the season is winter, the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 2-5.

[0013] Preferably, in the fire clay, the mass ratio of magnesia powder to resin is 4-8.

[0014] Preferably, the fire clay is prepared by the following method: a formulated amount of thermosetting resin and thermoplastic resin are mixed and stirred in a fire clay mixer, and a formulated amount of magnesia powder is continuously added thereto during the mixing and stirring process.

[0015] During the preparation of the present invention, the thermosetting resin and the thermoplastic resin are mixed evenly according to a ratio of 0.2 to 5. The ratio of the two resins is selected according to the season, that is, the temperature. In summer, when the ambient temperature is high, the two resins are selected to have a ratio of 0.2 to 2, and in winter, when the temperature is low, the two resins are selected to have a ratio of 2 to 5. First, the two resins that are evenly matched are added to the fire mud mixing mixer according to a certain amount, the mixer is turned on and the magnesia powder is continuously and slowly added to the mixer, and the stirring is stopped when the fire mud reaches a certain consistency but must have a certain fluidity. At this time, the fire mud can be evenly applied to the surface of the magnesia carbon brick and can be attached to the surface in a relatively short time without solidification or flow, which is the best degree.

[0016] When the present invention is used (i.e. during the process of laying magnesia carbon bricks at the bottom of the furnace), fire mud is applied around the magnesia carbon bricks with a thickness of 0.5-5 mm, and then the magnesia carbon bricks are squeezed and laid, that is, there is a 0.5-5 mm fire mud interval between the magnesia carbon bricks and they are firmly bonded together.

[0017] The present invention provides a fireclay for masonry of magnesia-carbon bricks at the active bottom of a converter. The technical solution selects an appropriate magnesia sand particle size so that the fireclay can maintain a stable thickness when applied; the use of two resins solves the problem of foaming when using thermoplastic resin alone and the problem of fast curing speed affecting the masonry process when using thermosetting resin alone. The use of two resins in combination not only overcomes the foaming of the fireclay but also alleviates the problem of fast curing affecting construction. The fireclay masonry allows the magnesia-carbon bricks at the bottom of the furnace to be carbonized by the heat during the converter steelmaking process to form a carbon chain structure, which absorbs the expansion of the magnesia-carbon bricks and allows the magnesia-carbon bricks at the bottom of the furnace to form a firmly bonded whole under the carbon chain structure of the fireclay, preventing the loosening and brick pulling accidents of the magnesia-carbon bricks at the bottom of the furnace, which is beneficial to ensure the safe use of the converter bottom and extend its service life. DETAILED DESCRIPTION

[0018] The specific embodiments of the present invention will be described in detail below. In order to avoid too much unnecessary details, the well-known structures or functions will not be described in detail in the following examples. The approximate language used in the following examples can be used for quantitative expression, indicating that the quantity can be allowed to have a certain change without changing the basic function. Unless otherwise defined, the technical and scientific terms used in the following examples have the same meaning as those generally understood by those skilled in the art to which the present invention belongs.

[0019] Example 1

[0020] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.3 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.5.

[0021] Example 2

[0022] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.5 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 4.

[0023] Example 3

[0024] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.2 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 2. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 1 mm.

[0025] Example 4

[0026] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.5 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 5. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 5 mm.

[0027] Example 5

[0028] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.3 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 1.25. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 3 mm.

[0029] Example 6

[0030] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 1.1. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 5 mm.

[0031] Example 7

[0032] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.2 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 1.3. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 1 mm.

[0033] Example 8

[0034] A fireclay for masonry of magnesia carbon bricks for active bottom of converter, characterized in that the fireclay contains magnesia sand powder and resin, the particle size of the magnesia sand powder is not greater than 0.2 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 0.6. The fireclay is retained between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 3 mm.

[0035] Example 9

[0036] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, the season is summer, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.2.

[0037] Example 10

[0038] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, the season is summer, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 1.

[0039] Embodiment 11

[0040] A fire clay for masonry of magnesia-carbon bricks for active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, the season is winter, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 4.

[0041] Example 12

[0042] A fire clay for masonry of magnesia-carbon bricks for active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, the season is winter, and the mass ratio of thermosetting resin to thermoplastic resin in the resin is 5.

[0043] Embodiment 13

[0044] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.4 mm, the resin contains thermosetting resin and thermoplastic resin, the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.9, and the mass ratio of the magnesia powder to the resin is 4.

[0045] Embodiment 14

[0046] A fire clay for laying magnesia-carbon bricks for the active bottom of a converter, characterized in that the fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.2 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 1.4. The mass ratio of magnesia powder to resin is 3.5. The fire clay is prepared by the following method: mixing and stirring the thermosetting resin and thermoplastic resin in a formula amount in a fire clay mixer, and continuously adding the magnesia powder in a formula amount during the mixing and stirring process.

[0047] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the scope of the present invention shall be included in the protection scope of the present invention.

Claims

1. A fire clay for laying magnesia carbon bricks for converter active bottom, characterized in that: The fire clay contains magnesia powder and resin, the particle size of the magnesia powder is not greater than 0.5 mm, the resin contains thermosetting resin and thermoplastic resin, and the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.2-5.

2. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 1, characterized in that: The fire clay is held between adjacent magnesia carbon bricks in a layered state, wherein the thickness of the layered state is 0.5 to 5 mm.

3. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 1, characterized in that: The particle size of the magnesia powder is not greater than 0.3 mm.

4. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 3, characterized in that: The fire clay is held between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 3 to 5 mm.

5. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 1, characterized in that: The particle size of the magnesia powder is not greater than 0.2 mm.

6. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 5, characterized in that: The fire mud is held between adjacent magnesia carbon bricks in a layered state, and the thickness of the layered state is 0.5 to 3 mm.

7. The fire clay for laying magnesia-carbon bricks for converter active bottom according to claim 1, characterized in that: When the season is summer, the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 0.2-2.

8. The fire clay for laying magnesia carbon bricks for converter active bottom according to claim 1, characterized in that: When the season is winter, the mass ratio of the thermosetting resin to the thermoplastic resin in the resin is 2-5.

9. The fire clay for laying magnesia carbon bricks for converter active bottom according to claim 1, characterized in that: In the fire clay, the mass ratio of magnesia powder to resin is 4-8.

10. The fire clay for laying magnesia carbon bricks for converter active bottom according to claim 1, characterized in that: The fire clay is prepared by the following method: a prescribed amount of thermosetting resin and a thermoplastic resin are mixed and stirred in a fire clay mixer, and a prescribed amount of magnesia powder is continuously added into the mixture during the mixing and stirring process.

Citation Information

Patent Citations

  • External stove integral production method for tapping hole brick of converter, and converter building method

    CN101430164A

  • Phenolic resin for magnesia carbon brick and preparation method thereof

    CN102219526A

  • Environmental-friendly magnesia carbon brick and production method thereof

    CN104844239A

  • Fire clay for cementing carbonic brick and preparation method thereof

    CN107117974A

  • Repairing material for tapping hole of converter and preparation method of repairing material

    CN117902906A