Thermal insulation layer and preparation method and application thereof
By using an insulation layer made of zirconia cement, the creep problem of platinum channels under high temperature and high current conditions was solved, ensuring the stability and clarification effect of platinum channels and improving the production efficiency of glass products.
Patent Information
- Application Number
- CN202411086122.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
AI Technical Summary
Platinum channels collapse and fracture due to the creep of alumina refractory cement under high temperature and high current conditions, affecting the clarification effect and reducing the pass rate of glass products.
Zirconia cement was used as the insulation layer material. The insulation layer was prepared by gradient sintering process, the particle size ratio of zirconia and alumina was controlled, and the mixture was filled between the platinum tube and the inner wall of the crucible to form a stable insulation layer structure.
It improves the high-temperature creep resistance of the platinum channel, preventing collapse and breakage, and enhancing the clarification effect and the pass rate of glass products.
Smart Images

Figure CN119019167A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal insulation materials, and in particular relates to a thermal insulation layer and a preparation method and application thereof. Background Art
[0002] The platinum channel is an important tool for preparing glass products. The main tasks of the platinum channel include clarifying the glass liquid, stirring the glass liquid, and adjusting the temperature of the glass liquid. The working principle of the platinum channel is: by applying voltage to the platinum flange electrodes welded at both ends of the platinum tube, current will flow through the platinum tube, thereby converting electrical energy into heat energy, thereby achieving the function of adjusting the temperature of the glass liquid.
[0003] However, the platinum tube needs to work continuously in a high temperature environment of up to 1200°C to 1670°C, and also needs to withstand a running current of up to several thousand amperes, which causes the strength of the platinum tube to drop sharply. In order to overcome this defect, the prior art is to place the platinum tube in a round or square corundum crucible, and fill the gap between the crucible and the platinum tube with alumina refractory cement, and support and cover the crucible with other refractory materials to form a heat-insulating environment.
[0004] Although the above method provides a certain degree of protection for the platinum tube, in the actual high-temperature operating environment, the staff found that the alumina refractory cement creeps under high-temperature conditions of about 800°C. This high-temperature creep phenomenon causes the outer side of the platinum channel to be squeezed by the alumina refractory cement. Coupled with the weight of the platinum channel itself, the platinum channel gradually collapses and deforms, greatly reducing the clarification effect of the platinum channel. In severe cases, the platinum channel may even break, causing significant losses to the production line. What is more serious is that after 12 months of operation using the above-mentioned platinum channel, the high-temperature creep problem of the alumina refractory cement will gradually worsen, and the degree of squeezing of the platinum tube will become more serious. After 18 months of operation, the platinum tube was squeezed and deformed by more than 30%, which seriously restricted the clarification efficiency of the platinum tube in the clarification area. Summary of the invention
[0005] The main purpose of the present invention is to provide a thermal insulation layer and a preparation method and application thereof. The technical problem to be solved is how to provide a preparation method of the thermal insulation layer that can effectively slow down the collapse or fracture of the platinum channel caused by being in a high temperature and high current working environment for a long time, thereby improving the clarification effect of the platinum channel and improving the qualified rate of glass products.
[0006] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. According to a method for preparing a thermal insulation layer proposed by the present invention, the method comprises: S1 mixing zirconia cement with water and stirring; in terms of mass percentage, the zirconia cement comprises: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the mass ratio of the zirconia cement to water is 2-3:1;
[0007] After S2 is evenly mixed, it is shaped and gradient sintered to obtain a thermal insulation layer; the gradient sintering includes: using a method of multiple heating to increase the temperature from room temperature to the sintering temperature.
[0008] Preferably, in the aforementioned preparation method, the method of multiple heating specifically comprises:
[0009] S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h;
[0010] S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃;
[0011] S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h;
[0012] S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h;
[0013] S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
[0014] Preferably, in the aforementioned preparation method, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0015] Preferably, in the aforementioned preparation method, the zirconia cement further comprises a rare earth metal.
[0016] The purpose of the present invention and the solution of its technical problems are also achieved by the following technical solutions. According to a thermal insulation layer proposed by the present invention, its raw materials include zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%.
[0017] Preferably, in the aforementioned thermal insulation layer, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0018] The purpose of the present invention and the solution to the technical problem are also achieved by the following technical solutions. A platinum channel proposed in the present invention comprises:
[0019] Crucible;
[0020] A platinum tube, the platinum tube is arranged in the crucible; the first electrode and the second electrode are arranged at both axial ends of the platinum tube; and,
[0021] The thermal insulation layer is embedded in and fills the gap between the platinum tube and the inner wall of the crucible; the raw material of the thermal insulation layer includes zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% of zirconium oxide and 5-20% of aluminum oxide; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the thickness of the thermal insulation layer is ≥5 mm.
[0022] Preferably, in the aforementioned platinum channel, the thickness of the thermal insulation layer is 5 mm to 50 mm; and / or the volume density of the thermal insulation layer is ≥ 2.5 g / cm 3 .
[0023] Preferably, in the aforementioned platinum channel, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0024] Preferably, in the aforementioned platinum channel, the raw materials of the crucible include, by mass percentage, 75% to 85% zirconium oxide, 15% to 20% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide.
[0025] The purpose of the present invention and the solution to the technical problem are also achieved by adopting the following technical solutions. According to a method for preparing a platinum channel proposed in the present invention, the method comprises the following steps:
[0026] S1: installing a platinum tube into the cavity of a crucible; a gap is left between the platinum tube and the crucible;
[0027] S2: Mixing zirconia cement with water, stirring, and then filling it into the gap, gradient sintering, and obtaining a thermal insulation layer; the mass ratio of the zirconia cement to water is 2-3:1; the thickness of the thermal insulation layer is 5mm-50mm; in terms of mass percentage, the zirconia cement includes: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1mm is 8%-20%; the gradient sintering includes: raising the temperature from room temperature to the sintering temperature by a method of multiple heating;
[0028] After the S3 gradient sintering is completed, electrodes are installed at both ends of the axial direction of the platinum tube to obtain a platinum channel.
[0029] Preferably, in the aforementioned preparation method, the raw materials of the crucible include, by mass percentage, 75% to 85% zirconium oxide, 15% to 20% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide.
[0030] Preferably, in the aforementioned preparation method, the components of the zirconia cement include, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide; and / or the electrical conductivity of the water is >2 megohms.
[0031] Preferably, in the aforementioned preparation method, the method of multiple heating specifically comprises:
[0032] S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h;
[0033] S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃;
[0034] S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h;
[0035] S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h;
[0036] S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
[0037] The purpose of the present invention and the technical problem solved are also achieved by adopting the following technical solutions: A glass manufacturing device proposed in the present invention includes the above-mentioned platinum channel.
[0038] By means of the above technical solution, the thermal insulation layer and the preparation method and application thereof proposed in the present invention have at least the following advantages:
[0039] The thermal insulation layer prepared by the present invention uses zirconia cement as the main production raw material, and the zirconia cement contains 80-95% zirconia and 5-20% alumina. Zirconia has an extremely high melting point, excellent thermal stability and thermal shock resistance, which enables the thermal insulation layer made of it to maintain structural integrity and stability in an extremely high temperature environment. The present invention also adjusts the proportion of zirconia cement in two key ranges of particle size of 0.01-0.5mm and particle size of 0.5-1mm by finely controlling the particle size distribution of zirconia cement in the raw material, that is, zirconia cement in two key ranges of particle size of 0.01-0.5mm and 0.5-1mm, so that the prepared thermal insulation layer has high temperature creep resistance, so that the thermal insulation layer will not creep due to being in a high temperature environment for a long time during use, thereby improving production efficiency.
[0040] In the preparation process of the insulation layer, the step-by-step heating method is used for sintering, which can remove excess water in the zirconia cement, so that the insulation layer has high-temperature creep resistance. The insulation layer is used on the outside of the platinum tube to avoid the collapse of the cement material due to creep, which compresses the deformation of the platinum tube, causing the platinum tube to reduce or fail to clarify the effect, and avoids the bubble defect caused by the glass liquid seeping out of the platinum tube, which reduces the clarification effect. The deformation of the insulation layer is ≤0.5%, and the strength at high temperature is ≥32kg.
[0041] The platinum channel prepared by the thermal insulation layer of the present invention can avoid the crucible and cement material collapse due to creep, which compresses the platinum tube and deforms it, causing the platinum tube to have a reduced clarification effect or fail. In addition, when the glass liquid seeps out of the platinum tube, it avoids the bubble defect caused by the glass liquid seeping out of the platinum tube, which reduces the clarification effect, thereby improving production efficiency.
[0042] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is a schematic diagram of the platinum channel structure of the present invention;
[0044] Figure 2 It is a left view of the platinum channel of the present invention. DETAILED DESCRIPTION
[0045] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description of a thermal insulation layer and its preparation method and application according to the present invention, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.
[0046] The present invention provides a method for preparing a thermal insulation layer, the method comprising: S1 mixing zirconia cement with water and stirring; the zirconia cement comprises, by mass percentage, 80-95% of zirconia and 5-20% of aluminum oxide; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the mass ratio of the zirconia cement to water is 2-3:1;
[0047] After S2 is evenly mixed, it is shaped and gradient sintered to obtain a thermal insulation layer; the gradient sintering includes: using a method of multiple heating to increase the temperature from room temperature to the sintering temperature.
[0048] The present invention uses zirconia cement with a particle size of 0.01-0.5 mm and 0.5-1 mm to ensure that the particles in the insulation layer are more evenly distributed, reduce the formation of pores and cracks, thereby effectively reducing heat loss and improving the insulation effect; and controlling the particle size of zirconia cement helps to form a more compact and stable insulation layer structure. Smaller particles can be filled in the gaps between large particles, reducing gaps and defects, thereby improving the overall strength and stability of the insulation layer.
[0049] On the basis of using zirconia cement with particle sizes of 0.01-0.5mm and 0.5-1mm, the present invention can make the insulation layer have better creep resistance under high temperature environment by accurately controlling the content of two different particle sizes of zirconia cement. This is because particles of different particle sizes have different deformation and creep rates at high temperatures, and the overall creep resistance can be improved through reasonable proportioning. In addition, it is also possible to fill the gaps between large particles of zirconia cement with an appropriate amount of smaller particles of zirconia cement, thereby reducing gaps and defects, improving the overall strength and stability of the insulation layer, and making the deformation of the insulation layer ≤0.5%, and the strength at high temperature ≥32kg.
[0050] In addition, the present invention can reduce production costs while ensuring the performance of the thermal insulation layer by optimizing the particle size ratio. Appropriate particle size distribution can reduce the waste of raw materials and improve the utilization rate of materials. Moreover, the zirconia cement material with appropriate particle size makes the thermal insulation layer material easier to operate during processing and construction. Appropriate particle size distribution can make the material more uniform, easy to mix and stir, thereby improving construction efficiency and quality.
[0051] The present invention controls the amount of water added because water is conductive. If the amount of water used is too much, the insulation of the thermal insulation layer will deteriorate during the heating process, which will cause the platinum tube to be grounded during use, resulting in bubbling of the glass in the platinum tube, thereby making the prepared glass product unqualified.
[0052] Preferably, in the aforementioned preparation method, the method of multiple heating specifically comprises:
[0053] S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h;
[0054] At the beginning of the preparation process, the insulation layer is heated from room temperature. The heating rate is controlled between 18℃ / h and 22℃ / h to ensure that the material can be heated evenly and avoid thermal stress caused by too fast or too slow heating. The heating time is between 5 and 7 hours depending on the heating rate.
[0055] S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃;
[0056] After reaching the target temperature of the first heating, the insulation layer needs to be kept at a temperature of 110℃~130℃ for a period of time, which is the insulation stage. The purpose of this stage is to fully dry the material, remove excess moisture, and stabilize the internal structure of the material. The insulation time is between 24 and 48 hours depending on the characteristics of the material and the preparation requirements.
[0057] S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h;
[0058] After the insulation stage, the insulation layer starts heating up for the second time. This time the heating rate is slower, controlled between 2℃ / h and 3℃ / h, to further stabilize the material structure and avoid thermal stress caused by too fast heating. The heating time is between 190 and 270 hours depending on the heating rate.
[0059] S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h;
[0060] After the second heating, the insulation layer enters the third heating stage. The heating rate this time is slightly faster than the second, but still controlled at a lower level (4-6℃ / h) to ensure that the material can be heated evenly. The heating time is between 67 and 100 hours depending on the heating rate.
[0061] S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
[0062] After the third heating, the insulation layer enters the final heating stage, which is also the highest temperature stage. The heating rate is faster this time, but still within the controllable range (7-9℃ / h) to ensure that the material can reach the required sintering temperature. The heating time is between 85 and 90 hours depending on the heating rate.
[0063] The entire preparation process ensures that the insulation layer can be heated evenly, removes excess moisture, stabilizes the internal structure, and ultimately reaches the required sintering temperature by precisely controlling the heating rate and insulation time, thereby improving the high-temperature stability and creep resistance of the insulation layer.
[0064] Preferably, in the aforementioned preparation method, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0065] Preferably, in the aforementioned preparation method, the zirconia cement further comprises a rare earth metal.
[0066] The present invention also proposes an insulation layer, the raw materials of which include zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% zirconium oxide and 5-20% aluminum oxide; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%.
[0067] Preferably, in the aforementioned thermal insulation layer, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0068] The present invention also proposes a platinum channel, such as Figure 1 and Figure 2 As shown, it includes:
[0069] Crucible 4;
[0070] A platinum tube 1, the platinum tube is arranged in the crucible; a first electrode 2 and a second electrode 5 are arranged at both axial ends of the platinum tube; and,
[0071] Insulation layer 3, the insulation layer is embedded in and fills the gap between the platinum tube and the inner wall of the crucible; the raw material of the insulation layer includes zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% zirconium oxide and 5-20% aluminum oxide; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the thickness of the insulation layer is ≥5mm.
[0072] The present invention uses a crucible as the main container of the platinum channel to accommodate the platinum tube and the insulation layer. The main materials of the crucible are zirconium oxide and aluminum oxide, wherein the content of zirconium oxide is ≥75% and the content of aluminum oxide is ≥15%; its material also includes silicon oxide ≤10% and iron oxide ≤0.1%. In the prior art, a corundum crucible is usually used, and the main component of the corundum crucible is aluminum oxide. Therefore, in a high temperature environment of 1600°C, the corundum crucible and the platinum channel will soften, and the softened corundum crucible will squeeze the softened platinum channel, causing the platinum tube to deform and reduce the clarification efficiency. The present invention uses a main material zirconium oxide with a content of ≥75%, which prevents the crucible from creeping during high temperature, thereby reducing the squeezing of the platinum channel and preventing the platinum tube from deforming during use.
[0073] The present invention limits the contents of zirconium oxide, aluminum oxide, silicon oxide and iron oxide in the crucible, so that the crucible can maintain excellent physical and chemical stability in a high-temperature environment of 1600°C, maintain structural integrity in a high-temperature environment, and is not easy to soften or deform during long-term operation of the platinum channel, so that the platinum tube will not be subjected to unnecessary extrusion during the heating process, effectively avoiding the problem of traditional corundum crucibles softening at high temperatures and squeezing the platinum channel, thereby reducing the clarification effect and improving production efficiency.
[0074] The crucible of the present invention is provided with an insulation layer inside, which is embedded in the gap between the platinum tube and the inner wall of the crucible and needs to fill the entire internal space of the crucible. The interior of the crucible is filled with insulation to effectively isolate the heat exchange of the external environment of the crucible, ensure that the temperature around the platinum tube is more stable and uniform, and is conducive to realizing accurate control of the temperature inside the platinum channel, thereby improving the qualified rate of the product.
[0075] The insulation layer of the present invention is wrapped around the outer surface of the platinum tube, and the thickness is controlled to be ≥5mm. The thickness of the insulation layer is not uniform, and the thickness of the insulation layer in some areas can be thicker and thinner in some areas. The minimum thickness of the insulation layer only needs to be 5mm.
[0076] Preferably, in the aforementioned platinum channel, the thickness of the thermal insulation layer is 5 mm to 50 mm; and / or the volume density of the thermal insulation layer is ≥ 2.5 g / cm 3 .
[0077] Preferably, in the aforementioned platinum channel, the zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
[0078] Preferably, in the aforementioned platinum channel, the raw materials of the crucible include, by mass percentage, 75% to 85% zirconium oxide, 15% to 20% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide.
[0079] The present invention also provides a method for preparing a platinum channel, which comprises the following steps:
[0080] S1: installing a platinum tube into the cavity of a crucible; a gap is left between the platinum tube and the crucible;
[0081] S2: Mixing zirconia cement with water, stirring, and then filling it into the gap, gradient sintering, and obtaining a thermal insulation layer; the mass ratio of the zirconia cement to water is 2-3:1; the thickness of the thermal insulation layer is 5mm-50mm; in terms of mass percentage, the zirconia cement includes: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1mm is 8%-20%; the gradient sintering includes: raising the temperature from room temperature to the sintering temperature by a method of multiple heating;
[0082] After the S3 gradient sintering is completed, electrodes are installed at both ends of the axial direction of the platinum tube to obtain a platinum channel.
[0083] Preferably, in the aforementioned preparation method, the raw materials of the crucible include, by mass percentage, 75% to 85% zirconium oxide, 15% to 20% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide.
[0084] Preferably, in the aforementioned preparation method, the components of the zirconia cement include, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide; and / or the electrical conductivity of the water is >2 megohms.
[0085] Water is conductive, therefore, the present invention limits the conductivity of water to > 2 megohms. If water with low conductivity is used, the insulation of the thermal insulation layer will deteriorate during the heating process, which may cause the platinum tube to be grounded during use, causing the glass in the platinum tube to bubble, thereby making the produced glass product unqualified.
[0086] Preferably, in the aforementioned preparation method, the method of multiple heating specifically comprises:
[0087] S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h;
[0088] S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃;
[0089] S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h;
[0090] S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h;
[0091] S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
[0092] The present invention also provides a glass manufacturing device, which comprises the above-mentioned platinum channel.
[0093] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0094] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.
[0095] Example 1
[0096] A method for preparing a thermal insulation layer comprises the following steps:
[0097] S1: Mixing zirconia cement with water and stirring; in terms of mass percentage, the zirconia cement comprises: 80% zirconia and 20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 80%; the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 20%; the mass ratio of the zirconia cement to water is 2:1;
[0098] After S2 is mixed evenly, it is shaped and gradient sintered, first raising the temperature from room temperature to 120°C, then to 900°C, and finally to 1600°C for sintering to obtain a thermal insulation layer; the thickness of the thermal insulation layer is 5mm; the gradient sintering includes: using a multiple heating method to raise the temperature from room temperature to the sintering temperature.
[0099] Example 2
[0100] Compared with Example 1, the added amounts of zirconium oxide and aluminum oxide in this example are as follows: in terms of mass percentage, the zirconium oxide cement comprises: 95% zirconium oxide and 5% aluminum oxide.
[0101] Example 3
[0102] Compared with Example 1, the added amounts of zirconium oxide and aluminum oxide in this example are as follows: in terms of mass percentage, the zirconium oxide cement comprises: 90% zirconium oxide and 10% aluminum oxide.
[0103] Example 4
[0104] Compared with Example 1, in this example, the zirconia cement includes, by mass percentage, 86.3% zirconium oxide, 8.5% aluminum oxide, 5% silicon oxide, 0.1% iron oxide and 0.1% carbonaceous matter.
[0105] Example 5
[0106] Compared with Example 1, the mass percentage of the zirconia cement with a particle size of 0.01-0.5 mm is 65%; the mass percentage of the zirconia cement with a particle size of 0.5-1 mm is 8%.
[0107] Example 6
[0108] Compared with Example 1, the mass percentage of the zirconia cement with a particle size of 0.01-0.5 mm is 70%; the mass percentage of the zirconia cement with a particle size of 0.5-1 mm is 15%.
[0109] Example 7
[0110] Compared with Example 6, the method of multiple heating in this embodiment includes:
[0111] S1 first heating: from room temperature to 120℃, the heating rate is 20℃ / h, and the heating time is 6h;
[0112] S2 insulation: insulation for 30 hours, insulation temperature is 120℃;
[0113] S3 second heating: heating to 500℃, heating rate is 2.5℃ / h, heating time is 230h;
[0114] S4 third heating: heating to 900℃, heating rate is 5℃ / h, heating time is 85h;
[0115] S5 fourth heating: heating to 1600°C, heating rate of 8°C / h, heating time of 87.5h.
[0116] Example 8
[0117] A method for preparing a platinum channel comprises the following steps:
[0118] S1: installing a platinum tube into the cavity of a crucible; a gap is left between the platinum tube and the crucible;
[0119] S2: Mixing zirconia cement with water, stirring, and then filling the gaps, gradient sintering, and obtaining a thermal insulation layer; the thickness of the thermal insulation layer is 5 mm; the zirconia cement comprises, by mass percentage, 80% zirconia and 20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 80%; the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 20%; the mass ratio of the zirconia cement to water is 2:1; the gradient sintering comprises: raising the temperature from room temperature to the sintering temperature by a method of multiple heating;
[0120] After the S3 gradient sintering is completed, electrodes are installed at both ends of the axial direction of the platinum tube to obtain a platinum channel.
[0121] Example 9
[0122] Compared with Example 8, the raw materials of the crucible and the raw materials of the insulation layer of this embodiment are as follows: in terms of mass percentage, the raw materials of the crucible include: 80% zirconium oxide, 16% aluminum oxide, 3.95% silicon oxide and 0.05% iron oxide; in terms of mass percentage, the components of the zirconium oxide cement include: 85% zirconium oxide, 8% aluminum oxide, 6.9% silicon oxide and 0.1% iron oxide.
[0123] Example 10
[0124] Compared with Example 9, the conductivity of the water used in this example is greater than 2 megohms.
[0125] Embodiment 11
[0126] Compared with Example 10, the method of multiple heating in this embodiment specifically includes:
[0127] S1 first heating: from room temperature to 120℃, the heating rate is 20℃ / h, and the heating time is 6h;
[0128] S2 insulation: insulation for 30 hours, insulation temperature is 120℃;
[0129] S3 second heating: heating to 500℃, heating rate is 2.5℃ / h, heating time is 230h;
[0130] S4 third heating: heating to 900℃, heating rate is 5℃ / h, heating time is 85h;
[0131] S5 fourth heating: heating to 1600°C, heating rate of 8°C / h, heating time of 87.5h.
[0132] Comparative Example 1
[0133] Compared with Example 1, in Comparative Example 1, only aluminum oxide was used as the raw material to prepare the thermal insulation layer.
[0134] Comparative Example 2
[0135] Compared with Example 5, in Comparative Example 2, the mass percentage of the zirconia cement with a particle size of 0.01 to 0.5 mm is 50%.
[0136] Comparative Example 3
[0137] Compared with Example 5, in Comparative Example 3, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 85%.
[0138] Comparative Example 4
[0139] Compared with Example 5, in Comparative Example 4, the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 25%.
[0140] Comparative Example 5
[0141] Compared with Example 5, in Comparative Example 5, the mass percentage of the zirconia cement with a particle size of 0.5 to 1 mm is 5%.
[0142] Comparative Example 6
[0143] Compared with Example 5, in Comparative Example 6, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 90%; the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 5%.
[0144] Comparative Example 7
[0145] Compared with Example 5, in Comparative Example 7, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 60%; the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 30%.
[0146] Comparative Example 8
[0147] Compared with Example 8, the thermal insulation layer used in Comparative Example 8 is the thermal insulation layer described in Comparative Example 1.
[0148] The thermal insulation layers prepared in Examples 1 to 7 were placed in a high temperature environment of about 800°C to observe whether the thermal insulation layers had creep phenomena and to test their strength. The specific detection method is:
[0149] The method for detecting the deformation of the insulation layer is:
[0150] S1 Process the samples of Examples 1 to 7 and Comparative Examples 1 to 7 into standard blocks with a length, width and height of 5 cm, and record the initial volume V of the standard block 1 ;
[0151] S2 places the standard block in a high temperature environment of 800℃ for sintering. After sintering, the volume V of the sintered standard block is accurately measured. 2 , and then calculate by the formula:
[0152] F=(V 1 -V 2 ) / V 1
[0153] Where, F is the deformation, in %; V 1 is the initial volume of the standard block, in cm 3 ; V 2 is the volume of the standard block after sintering, in cm 3 .
[0154] The testing method for high temperature strength of the insulation layer is:
[0155] S1 Process the samples of Examples 1 to 7 and Comparative Examples 1 to 7 into standard blocks with a length, width and height of 5 cm;
[0156] S2 places the standard block in a high temperature environment of 800°C for sintering;
[0157] After S3 sintering is completed, weights of different masses are applied to the standard block one by one until it can no longer withstand the pressure and breaks. The weights are weighed to obtain the strength at high temperature in kg.
[0158] The results are as follows:
[0159] Table 1
[0160] Example Deformation (%) Strength at high temperature (kg) Example 1 0.42 34.0 Example 2 0.40 34.7 Example 3 0.43 33.5 Example 4 0.19 36.1 Example 5 0.46 32.9 Example 6 0.22 35.2 Example 7 0.15 36.6 Comparative Example 1 7.60 11.6 Comparative Example 2 0.71 29.7 Comparative Example 3 0.66 30.0 Comparative Example 4 1.20 27.3 Comparative Example 5 3.60 22.0 Comparative Example 6 0.90 28.8 Comparative Example 7 0.54 31.0
[0161] It can be seen from the test data in Table 1 that the technical solution proposed in the present invention, such as Examples 1 to 7, is used to make an insulation layer made of a specific ratio of zirconia cement containing 80 to 95% zirconia and 5 to 20% alumina. By controlling the ratio of cement particle size, the insulation layer exhibits excellent structural integrity and stability in an extremely high temperature environment, with a deformation of ≤0.5%, only 0.42%, and a strength of ≥32 kg at high temperature, as high as 34.0 kg, which is significantly better than Comparative Example 1.
[0162] Comparing the data of Example 5 with Comparative Examples 2 to 7, Example 5 finely controls the particle size distribution of zirconia cement. Specifically, the proportion of cement with a particle size of 0.01 to 0.5 mm is controlled at 65 to 80%, and that of cement with a particle size of 0.5 to 1 mm is controlled at 8 to 20%. Finely controlling the particle size distribution of zirconia cement in the present invention can give the insulation layer excellent high-temperature creep resistance. Even if exposed to high temperature for a long time, the insulation layer can maintain a stable shape, effectively avoiding creep, thereby improving overall production efficiency and reliability.
[0163] As can be seen from Example 6, the present invention further optimizes the particle size of zirconia cement, selecting cement with a particle size of 0.01-0.5 mm to account for 70%, and cement with a particle size of 0.5-1 mm to account for 15%. This precise ratio can reduce the deformation of the insulation layer under extreme conditions to 0.22%, and increase the high temperature strength to 35.2 kg.
[0164] It can be seen from Example 7 that based on the better particle size optimization of Example 6, the multiple heating process is improved and a more sophisticated temperature control strategy is adopted to reduce the deformation of the insulation layer under extreme conditions to 0.15%, while the strength at high temperature is increased to 36.6k.
[0165] The platinum channels prepared in Examples 8 to 9 were placed in a high temperature environment of about 800°C for operation for 18 months to observe whether the platinum tube was deformed. The specific detection method was as follows: the diameter height of the platinum tube was measured before the equipment was used, and the diameter height of the platinum tube was measured after use. The height changes were compared to determine whether deformation occurred.
[0166] The results are as follows:
[0167]
[0168] By comparing Example 8 with Comparative Example 8, it can be seen that after running at 800°C for 18 months, the platinum channel obtained in Example 8 has only undergone slight deformation. This is because in Example 8, a traditional alumina crucible was selected as a container. After 18 months of use, the crucible collapsed. This collapse phenomenon not only directly squeezes the built-in insulation layer, but also indirectly affects the platinum tube. Comparative Example 8 not only uses an alumina crucible, but also an alumina insulation layer. When the platinum tube is running at high temperature, the outer side is squeezed by the alumina refractory cement and affected by its own weight, and it will gradually collapse and deform. In severe cases, it will break, causing serious damage and failure of the production line.
[0169] When comparing Example 8 with Example 9, it can be found that Example 9 adopts a special crucible design and cleverly combines a platinum channel layout coordinated with the insulation layer. During the same 18-month service life, the platinum tube of the platinum channel does not deform, which greatly improves the service life of the product and production efficiency.
[0170] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0171] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a thermal insulation layer, It is characterized in that It includes the following steps: S1. Mix zirconia cement and water and stir; In terms of mass percentage, the zirconia cement comprises: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the mass ratio of the zirconia cement to water is 2-3:1; After S2 is evenly mixed, it is shaped and gradient sintered to obtain a thermal insulation layer; the gradient sintering includes: using a method of multiple heating to increase the temperature from room temperature to the sintering temperature.
2. The preparation method according to claim 1, It is characterized in that The method of multiple temperature increases specifically includes: S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h; S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃; S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h; S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h; S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
3. The preparation method according to claim 1, It is characterized in that The zirconia cement comprises, by mass percentage, 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter; and / or the zirconia cement further comprises rare earth metals.
4. A thermal insulation layer, It is characterized in that The raw materials include zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% of zirconia and 5-20% of aluminum oxide; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%.
5. The thermal insulation layer according to claim 4, It is characterized in that Calculated by mass percentage, the zirconia cement comprises: 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter.
6. A platinum channel, It is characterized in that It includes: Crucible; A platinum tube, the platinum tube is disposed in the crucible; The platinum tube is provided with a first electrode and a second electrode at two axial ends; and, A heat-insulating layer, the heat-insulating layer is embedded in and fills the gap between the platinum tube and the inner wall of the crucible; The raw material of the thermal insulation layer includes zirconia cement; in terms of mass percentage, the zirconia cement includes: 80-95% zirconia and 5-20% alumina; In the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01 to 0.5 mm is 65% to 80%; the mass percentage of zirconia cement with a particle size of 0.5 to 1 mm is 8% to 20%; the thickness of the thermal insulation layer is ≥5 mm.
7. The platinum channel according to claim 6, It is characterized in that The thickness of the thermal insulation layer is 5 mm to 50 mm; and / or the volume density of the thermal insulation layer is ≥ 2.5 g / cm 3 ; and / or, in terms of mass percentage, the zirconia cement comprises: 80% to 90% zirconia, 5% to 10% alumina, 0% to 10% silica, 0% to 0.1% iron oxide and 0% to 0.1% carbonaceous matter; and / or, in terms of mass percentage, the raw materials of the crucible comprise: 75% to 85% zirconia, 15% to 20% alumina, 0% to 10% silica and 0% to 0.1% iron oxide.
8. A method for preparing a platinum channel, It is characterized in that It includes the following steps: S1: installing a platinum tube into the cavity of a crucible; a gap is left between the platinum tube and the crucible; S2: mixing zirconia cement with water, stirring, and then filling the mixture into the voids, and gradient sintering to obtain a thermal insulation layer; the mass ratio of the zirconia cement to water is 2 to 3:1; and the thickness of the thermal insulation layer is 5 mm to 50 mm; In terms of mass percentage, the zirconia cement comprises: 80-95% zirconia and 5-20% alumina; in the zirconia cement, the mass percentage of zirconia cement with a particle size of 0.01-0.5 mm is 65%-80%; the mass percentage of zirconia cement with a particle size of 0.5-1 mm is 8%-20%; the gradient sintering comprises: raising the temperature from room temperature to the sintering temperature by a multiple heating method; After the S3 gradient sintering is completed, electrodes are installed at both ends of the axial direction of the platinum tube to obtain a platinum channel.
9. The preparation method according to claim 8, It is characterized in that In terms of mass percentage, the raw materials of the crucible include: 75% to 85% zirconium oxide content, 15% to 20% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide; and / or, in terms of mass percentage, the components of the zirconium oxide cement include: 80% to 90% zirconium oxide, 5% to 10% aluminum oxide, 0% to 10% silicon oxide and 0% to 0.1% iron oxide; and / or, the conductivity of the water is greater than 2 megohms; and / or, the method of multiple heating specifically includes: S1 first heating: from room temperature to 110℃~130℃, the heating rate is 18℃ / h~22℃ / h, and the heating time is 5h~7h; S2 insulation: insulation for 24h~48h, insulation temperature is 110℃~130℃; S3 second heating: heating to 490℃~510℃, heating rate is 2℃ / h~3℃ / h, heating time is 190~270h; S4 third heating: heating to 890℃~910℃, heating rate is 4℃ / h~6℃ / h, heating time is 67h~100h; S5 fourth heating: heating to 1590℃~1610℃, heating rate is 7℃ / h~9℃ / h, heating time is 85h~90h.
10. A glass manufacturing device, It is characterized in that It comprises the platinum channel as claimed in claim 6 or 7.