Synthesis method of low-dielectric hydrocarbon resin
By reacting styrene with second monomer and other substances under an inert gas atmosphere and adding vinyl magnesium bromide to form a low-dielectric hydrocarbon resin, the insufficient mechanical strength and thermal performance of hydrocarbon resin in high-frequency and high-speed circuits is solved. The problem of this achieves the effect of low dielectric constant and high glass transition temperature.
Patent Information
- Application Number
- CN202411165116.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
The existing hydrocarbon resins have problems with low mechanical strength and insufficient thermal performance in high-frequency and high-speed circuit applications, and the prior art is difficult to meet the requirements of higher and lower dielectric materials, especially in the high-temperature welding process.
Injector, styrene, second monomer, molecular weight regulator and solvent are mixed with the inert gas atmosphere, and vinyl magnesium bromide is added after the reaction, and a low dielectric hydrocarbon resin is formed through cross-linking reaction, and the synthesis process is adjusted. Vinyl content to obtain resins of different glass transition temperatures.
Hydrocarbon resins with low dielectric constant (not exceeding 2.5), low dielectric loss (not exceeding 0.0005) and high glass transition temperature (not below 130°C) are achieved, which improves the mechanical strength and high temperature resistance of the material.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resin synthesis, and in particular relates to a method for synthesizing a low-dielectric hydrocarbon resin containing a styrene structure. Background Art
[0002] In recent years, the vigorous development of industries such as 5G communication technology, the Internet of Things, and new energy vehicles has promoted the transformation and upgrading of the copper clad laminate industry to high frequency and high speed, prompting the matrix resin adapted to high-frequency applications to become the key research direction of today's material manufacturers. Among them, hydrocarbon resin has good low dielectric and low loss properties due to its extremely low molecular polarity, making it a high-frequency and high-speed copper clad laminate substrate with extremely low / ultra-low loss (dielectric loss Df<0.008). However, as a thermoplastic resin, hydrocarbon resin can flow and deform after being heated, and has problems such as low mechanical strength and insufficient thermal performance. Therefore, it is necessary to enhance and modify it, and form a highly cross-linked interpenetrating polymer network structure through the cross-linking reaction of unsaturated double bonds in the molecule, so that it can be transformed from a thermoplastic to a thermosetting resin, thereby improving the mechanical strength and high temperature resistance of hydrocarbon resin materials.
[0003] There are two mainstream resin composition process routes for copper clad laminates used in high-frequency and high-speed circuits with low loss level or above (substrate Df≤0.008): one is a process route composed of thermoplastic resin systems represented by polytetrafluoroethylene (PTFE); the other is a process route composed of thermosetting resin systems represented by modified polyphenylene ether resins.
[0004] In the early stages of the development of high-frequency and high-speed substrate materials, PTFE resin became the earliest and most mature special resin to be used because it is easy to achieve low dielectric loss, but its industrialization cost is relatively high. In addition, because it is a thermoplastic resin, PTFE faces many difficulties in terms of process and equipment matching in realizing the multi-layering of antenna substrates and the composite structure of substrates. The dielectric properties of polyphenylene ether (PPO, dielectric constant: 2.6-2.8; dielectric loss: 0.008-0.0042) are the smallest among engineering plastics, and the processability of PPO materials is much better than that of PTFE materials. Therefore, in the second process route composed of thermosetting resin systems, "PPO as the main body + cross-linking agent (the cross-linking agent can be bismaleimide resin, triallyl triisocyanate TAIC, hydrocarbon resin, etc.)" is currently the mainstream route. At the same time, the resin composition design technology for copper clad laminates for high-frequency and high-speed circuits has been continuously advanced in recent years. There have emerged process routes with modified maleimide (difunctional and multi-functional types) as the main resin; very low loss (Very Low Loss) grades composed of special epoxy resins (dicyclopentadiene type, diphenyl ether type, etc.) + benzoxazine resin process routes, as well as copper clad laminate varieties with high-frequency and high-speed circuit substrates below the very low loss level.
[0005] However, as equipment requirements continue to increase, polyphenylene ether is gradually unable to meet the requirements of higher low dielectric materials, and the process route consisting of thermosetting resin systems represented by hydrocarbon resins has gradually been studied.
[0006] At present, the commonly used hydrocarbon resins are mostly diene polymers, such as polybutadiene, polyisoprene, or polybutadiene-polystyrene copolymers. Diene polymers have low dielectric constants and dielectric losses, but these materials have low temperature resistance. Electrical insulating materials such as copper-clad laminates are exposed to high-temperature reflow soldering during the soldering of components, so resins need to have heat resistance, that is, materials that show a high glass transition temperature. In particular, due to environmental issues, lead-free solders with high melting points are used recently, so the requirements for electrical insulating materials with higher heat resistance are increasing. In response to these requirements, it has been proposed to use hardened resins of vinyl compounds with various chemical structures.
[0007] Thermosetting polystyrene has low density: 1.05g / cm³, only half of polytetrafluoroethylene; stable dielectric properties: dielectric constant is 2.5, loss factor is as low as 0.0004, and dielectric properties are stable and do not change significantly at different frequencies (especially at 1MHz~500GHz); good rigidity and dimensional stability: no permanent deformation or plastic flow, internal stress relief has been carried out during production and preparation, and no stress relief is required in later use; glass transition temperature increases with the increase of crosslinking density, excellent chemical resistance: good chemical resistance to acid, alkali, salt solution, aliphatic hydrocarbon solvents; suitable for microwave lenses and precision parts, microwave circuits, antennas, coaxial cable connectors, sound sensors, satellite antennas, sonar lenses, non-destructive material testing devices, monitoring equipment, radar windows, radar covers and missile guidance system shells and large energy equipment, high-power pulse equipment, etc. There is no literature reporting the synthesis method.
[0008] Based on this, this application was developed. Summary of the invention
[0009] The present invention aims to overcome the defects of the prior art and provides a method for synthesizing a low dielectric hydrocarbon resin containing a styrene structure. The hydrocarbon resin synthesized by the method has a lower dielectric constant and node loss and a higher glass transition temperature.
[0010] To achieve the above object, the present invention adopts the following technical solution: A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: In an inert gas atmosphere (such as nitrogen, argon or helium), the initiator, styrene, the second monomer, the molecular weight regulator and the solvent are mixed and reacted at 60-120°C for 2-6 hours. After the reaction liquid is cooled to room temperature, vinyl magnesium bromide is added, and then reacted at 20-60°C for 1-10 hours. After the reaction is completed, the low dielectric hydrocarbon resin solution is obtained by washing with water.
[0011] In the above-mentioned synthesis method, specifically, by weight, 0.05-1 parts of an initiator, 100 parts of styrene, 5-20 parts of a second monomer, 0-10 parts of a molecular weight regulator, and 100-500 parts of a solvent may be added, preferably reacting at 100-120° C. for 3-6 hours. After cooling to room temperature, 15-30 parts by weight of vinyl magnesium bromide may be added.
[0012] Furthermore, the initiator may be one or a mixture of two or more of azobisisobutyronitrile (AIBN), dibenzoyl peroxide, dicumyl peroxide, etc.
[0013] Furthermore, the second monomer may be one or a mixture of two or more of 4-chlorostyrene, 2-chlorostyrene, 6-chlorostyrene, 4-bromostyrene, 2-bromostyrene, 6-bromostyrene and the like.
[0014] Furthermore, the molecular weight regulator may be 2,4-diphenyl-4-methyl-1-pentene or the like.
[0015] Furthermore, the solvent may be one or a mixture of two or more of toluene, xylene, ethyl acetate, butyl acetate, N,N-dimethylformamide, etc.
[0016] The present invention also provides a low dielectric hydrocarbon resin synthesized by the above synthesis method. The process route of the synthesis method of the present invention is as follows, wherein R is -Cl, -Br, etc.
[0017] .
[0018] Compared with the prior art, the beneficial effects of the synthesis method of the present invention are as follows: The present invention discloses a method for synthesizing a low dielectric hydrocarbon resin containing a styrene structure. During the synthesis process, polystyrene is mainly a hydrocarbon structure, and the exposed vinyl has a high reactivity. By adjusting the vinyl content, resins with different glass transition temperatures are obtained. The hydrocarbon resin synthesized by the method has a low dielectric constant (dielectric constant not exceeding 2.5), a dielectric loss (dielectric loss not exceeding 0.0005), and a high glass transition temperature (glass transition temperature not less than 130°C). BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the GPC spectrum of the product synthesized in Example 1. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is further described in detail below in conjunction with the embodiments, but the protection scope of the present invention is not limited thereto.
[0021] In the following examples, the raw materials used are all common commercial products that can be directly purchased or can be prepared by conventional methods in the art.
[0022] Unless otherwise specified, room temperature refers to 25±5℃.
[0023] Example 1 A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: Nitrogen was introduced into a three-necked flask. Under nitrogen atmosphere, 0.5 g of diisopropylbenzene peroxide, 100 g of styrene, 10 g of 4-chlorostyrene, 5 g of 2,4-diphenyl-4-methyl-1-pentene and 100 g of toluene were added. The mixture was reacted at 120°C for 3 h. After the reaction solution was cooled to room temperature, 15 g of vinylmagnesium bromide was added. The mixture was reacted at 20°C for 4 h. After the reaction was completed, 100 ml of water was added in five portions. The mixture was allowed to stand for stratification. The water layer was removed and the mixture was washed with water for 3 times to obtain a light yellow toluene solution of a hydrocarbon resin containing a styrene structure.
[0024] Figure 1 The GPC spectrum of the synthesized hydrocarbon resin containing styrene structure in toluene solution is given. Figure 1 As shown in the figure, it can be seen that the monomer is polymerized and presents a single peak with a molecular weight of 30,000. Using a vector network analyzer to test: the dielectric constant is 2.5, the dielectric loss is 0.0004, and the glass transition temperature (Tg) is 130°C.
[0025] Example 2 A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: Nitrogen was introduced into a three-necked flask. Under nitrogen atmosphere, 1 g of diisopropylbenzene peroxide, 100 g of styrene, 20 g of 4-bromostyrene, 10 g of 2,4-diphenyl-4-methyl-1-pentene and 500 g of xylene were added. The mixture was reacted at 100°C for 4 h. After the reaction solution was cooled to room temperature, 20 g of vinylmagnesium bromide was added. The mixture was reacted at 20°C for 4 h. After the reaction was completed, 100 ml of water was added in five portions. The mixture was allowed to stand for stratification. The water layer was removed and the mixture was washed with water for 3 times to obtain a light yellow xylene solution of a hydrocarbon resin containing a styrene structure.
[0026] The toluene solution of the synthesized hydrocarbon resin containing styrene structure was tested, and the results showed that the molecular weight was 10,000, the dielectric constant was 2.47, the dielectric loss was 0.00037, and the glass transition temperature (Tg) was 150°C.
[0027] Example 3 A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: Nitrogen was introduced into a three-necked flask. Under nitrogen atmosphere, 0.2 g of azobisisobutyronitrile, 100 g of styrene, 15 g of 4-bromostyrene, 8 g of 2,4-diphenyl-4-methyl-1-pentene and 500 g of toluene were added. The mixture was reacted at 110°C for 3 h. After the reaction solution was cooled to room temperature, 30 g of vinylmagnesium bromide was added. The mixture was reacted at 20°C for 4 h. After the reaction was completed, 100 ml of water was added in five portions. The mixture was allowed to stand for stratification. The water layer was removed and the mixture was washed with water for 3 times to obtain a light yellow xylene solution of a hydrocarbon resin containing a styrene structure.
[0028] The toluene solution of the synthesized hydrocarbon resin containing styrene structure was tested, and the results showed that the molecular weight was 17,000, the dielectric constant was 2.5, the dielectric loss was 0.00041, and the glass transition temperature (Tg) was 142°C.
[0029] Example 4 A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: Nitrogen was introduced into a three-necked flask. Under nitrogen atmosphere, 0.1 g of dibenzoyl peroxide, 100 g of styrene, 12 g of 2-bromostyrene, 6 g of 2,4-diphenyl-4-methyl-1-pentene and 200 g of butyl acetate were added. The mixture was reacted at 110°C for 3 h. After the reaction solution was cooled to room temperature, 20 g of vinylmagnesium bromide was added. The mixture was reacted at 40°C for 3 h. After the reaction was completed, 100 ml of water was added in five portions. The mixture was allowed to stand for stratification. The water layer was removed and the mixture was washed with water for 3 times to obtain a light yellow xylene solution of a hydrocarbon resin containing a styrene structure.
[0030] The toluene solution of the synthesized hydrocarbon resin containing styrene structure was tested and the results showed that the molecular weight was 30,000, the dielectric constant was 2.47, the dielectric loss was 0.00042, and the glass transition temperature (Tg) was 137°C.
[0031] Example 5 A method for synthesizing a low dielectric hydrocarbon resin comprises the following steps: Nitrogen was introduced into a three-necked flask. Under nitrogen atmosphere, 0.8 g of azobisisobutyronitrile, 100 g of styrene, 14 g of 6-chlorostyrene, 8 g of 2,4-diphenyl-4-methyl-1-pentene and 400 g of N,N-dimethylformamide were added. The mixture was reacted at 110°C for 3 h. After the reaction solution was cooled to room temperature, 20 g of vinylmagnesium bromide was added. The mixture was reacted at 40°C for 3 h. After the reaction was completed, 100 ml of water was added in five portions. The mixture was allowed to stand for stratification. The water layer was removed and the mixture was washed with water for 3 times to obtain a light yellow xylene solution of a hydrocarbon resin containing a styrene structure.
[0032] The toluene solution of the synthesized hydrocarbon resin containing styrene structure was tested, and the results showed that the molecular weight was 29,000, the dielectric constant was 2.48, the dielectric loss was 0.00041, and the glass transition temperature (Tg) was 139°C.
Claims
1. A method for synthesizing a low dielectric hydrocarbon resin, characterized in that: The steps include: In an inert gas atmosphere, the initiator, styrene, the second monomer, the molecular weight regulator and the solvent are mixed, reacted at 60-120°C for 2-6 hours, cooled to room temperature, vinyl magnesium bromide is added, and then reacted at 20-60°C for 1-10 hours. After the reaction is completed, the mixture is washed with water to obtain a low dielectric hydrocarbon resin solution.
2. The method for synthesizing a low dielectric hydrocarbon resin according to claim 1, characterized in that: In parts by weight, 0.05-1 parts of an initiator, 100 parts of styrene, 5-20 parts of a second monomer, 0-10 parts of a molecular weight regulator, and 100-500 parts of a solvent are added.
3. The method for synthesizing a low dielectric hydrocarbon resin as claimed in claim 2, characterized in that: Add 15-30 parts by weight of vinyl magnesium bromide.
4. The method for synthesizing a low dielectric hydrocarbon resin according to claim 1, characterized in that: The initiator is one of azobisisobutyronitrile, dibenzoyl peroxide and dicumyl peroxide, or a mixture of two or more thereof.
5. The method for synthesizing a low dielectric hydrocarbon resin according to claim 1, characterized in that: The second monomer is one of 4-chlorostyrene, 2-chlorostyrene, 6-chlorostyrene, 4-bromostyrene, 2-bromostyrene, and 6-bromostyrene, or a mixture of two or more thereof.
6. The method for synthesizing a low dielectric hydrocarbon resin according to claim 1, characterized in that: The molecular weight regulator is 2,4-diphenyl-4-methyl-1-pentene.
7. The method for synthesizing a low dielectric hydrocarbon resin according to claim 1, characterized in that: The solvent is one or a mixture of two or more of toluene, xylene, ethyl acetate, butyl acetate, and N,N-dimethylformamide.
8. The method for synthesizing a low dielectric hydrocarbon resin as claimed in claim 1, characterized in that: Under nitrogen, argon or helium atmosphere.
9. A low dielectric hydrocarbon resin synthesized by the synthesis method according to any one of claims 1 to 8.