Bio-based polyurethane elastomer as well as preparation method and application thereof

By performing addition polymerization in a specific ratio of bio-based polyol, 1,5-pentadiisocyanate and 1,3-propylene glycol, a bio-based polyurethane elastomer with excellent mechanical properties and stability is formed, and through renewable cycles The use of the process to reduce costs has solved the problems of poor mechanical properties and non-recyclable utilization of bio-based polyurethane elastomers in the prior art, and achieved low-cost large-scale production and environmentally friendly applications.

CN119019641AInactive Publication Date: 2024-11-26FUDAN UNIVERSITY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411514991.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing bio-based polyurethane elastomers have shortcomings in terms of mechanical properties, recycling properties and costs, which limit their application in the market.

Method used

By performing addition polymerization reaction in a specific ratio of bio-based polyol, 1,5-pentadiisocyanate and 1,3-propylene glycol, a bio-based polyurethane elastomer with excellent elasticity and toughness, it forms uniform and stable through vulcanization reaction The network structure improves mechanical performance while designing a renewable recycling process to reduce costs.

Benefits of technology

It achieves excellent mechanical properties and stability of bio-based polyurethane elastomers, and still maintains load bearing capacity and initial mechanical properties after 5 recycling cycles. It has good environmental friendliness and low cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019641A_ABST
    Figure CN119019641A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-based polyurethane elastomer as well as a preparation method and application thereof, and belongs to the technical field of high polymer materials. The bio-based polyurethane elastomer provided by the invention is prepared by carrying out addition polymerization reaction on 45-75 parts by mass of bio-based polyol, 3-8 parts by mass of 1, 3-propylene glycol and 22-47 parts by mass of 1, 5-pentamethylene diisocyanate, and the mass sum of the 1, 5-pentamethylene diisocyanate and the 1, 3-propylene glycol accounts for 25-55% of the total mass of the raw materials. The content of 1, 5-pentamethylene diisocyanate and 1, 3-propylene glycol is limited, so that the mechanical property and the stability of bio-based polyurethane can be effectively improved, the bio-based polyurethane can be regenerated after simple treatment, after five times of recycling, the initial mechanical property and the excellent load bearing capacity are still kept, the excellent recoverable and recyclable use performance is shown, and the method is suitable for industrial production. The composite material is widely applied to building materials, automobile accessories, medical facilities, medical instruments and textile materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of polyurethane elastomer materials, and in particular relates to a bio-based polyurethane elastomer and a preparation method and application thereof. Background Art

[0002] Bio-based polyurethane elastomers are made from renewable raw materials, have good biodegradability, are cheap and environmentally friendly, and are an important direction for future development. However, existing bio-based polyurethane elastomers are prepared using polyols and isocyanates, and due to the influence of the ratio and reaction conditions, they have poor mechanical properties, which limits their application in the market. Therefore, it is necessary to modify bio-based polyurethane elastomers to improve their comprehensive properties.

[0003] At present, in the related art, a chain extending cross-linking agent is generally added to a polyurethane prepolymer to give the bio-based polyurethane elastomer excellent mechanical and thermal properties. For example, the prior art with application publication number CN 111393604 A discloses a polyurethane elastomer, which is prepared by adding a mixed chain extending cross-linking agent to a polyurethane prepolymer to obtain a polyurethane elastomer with a tensile strength of 50-52 MPa.

[0004] However, the polyurethane elastomers modified by the existing methods have the following problems: first, due to the addition of chain extenders and crosslinkers, the mechanical properties of the polyurethane elastomers are poor, and the hardness, elasticity and durability cannot be met at the same time; second, they do not have the ability to be recycled and reused, resulting in a waste of resources; third, the raw material cost is high, which is not conducive to large-scale production. Summary of the invention

[0005] The present application discloses a bio-based polyurethane elastomer and a preparation method and application thereof, aiming to solve the technical problems of existing polyurethane elastomers such as poor mechanical properties, non-recyclability and high cost.

[0006] In order to achieve the above purpose, the technical solution of this application is:

[0007] The first aspect of the present application provides a bio-based polyurethane elastomer, which is prepared by addition polymerization of raw materials comprising the following components:

[0008] 45-75 parts by weight of bio-based polyol;

[0009] 22-47 parts by mass of 1,5-pentanediisocyanate;

[0010] 3-8 parts by mass of 1,3-propylene glycol;

[0011] The bio-based polyol is bio-based 1,4-butanediol or A polyol;

[0012] The A polyol is prepared by esterification and polycondensation of 1,3-propylene glycol and a dibasic acid;

[0013] The mass of the 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 25-55% of the total mass of the raw materials.

[0014] In combination with the first aspect, preferably, the total mass of the 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 40% of the total mass of the raw materials.

[0015] In combination with the first aspect, preferably, the A polyol is prepared by a method comprising the following steps:

[0016] 1,3-propylene glycol, dibasic acid and tetrabutyl titanate are mixed for esterification reaction, and the temperature is raised for polycondensation reaction to obtain polyol A;

[0017] The molecular weight of the A polyol is 80,000-100,000 g / mol.

[0018] In combination with the first aspect, preferably, the dibasic acid is one of sebacic acid, adipic acid and dodecanedioic acid.

[0019] The second aspect of the present application provides a method for preparing the bio-based polyurethane elastomer according to the first aspect, the preparation method comprising:

[0020] The bio-based polyol and 1,5-pentanediisocyanate are reacted to generate a prepolymer, and then 1,3-propylene glycol is added to carry out a vulcanization reaction to obtain the bio-based polyurethane elastomer.

[0021] In combination with the second aspect, preferably, the temperature of the vulcanization reaction is 60-90°C.

[0022] In combination with the second aspect, preferably, the sulfurization reaction time is 2-4 h.

[0023] The third aspect of the present application provides the use of the bio-based polyurethane elastomer described in the first aspect or the bio-based polyurethane elastomer prepared by the preparation method described in the second aspect in building materials, public facilities, medical facilities and medical equipment, and textile materials.

[0024] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:

[0025] The bio-based polyurethane elastomer provided by the present application uses bio-based polyol as the soft segment, 1,5-pentamethylene diisocyanate and 1,3-propylene glycol as the hard segment, and controls the hard segment to undergo addition polymerization reaction at a specific content. On the one hand, it can effectively regulate the microphase separation structure of the hard segment and the soft segment, so that the bio-based polyurethane elastomer has excellent elasticity and toughness while having excellent mechanical properties and stability; on the other hand, the bio-based polyurethane elastomer prepared by the present application can be regenerated after simple treatment, and after 5 recycling cycles, it can still maintain excellent load-bearing capacity and initial mechanical properties, and has good environmental friendliness; in addition, the raw materials are renewable bio-based materials, which are low in cost, can be mass-produced, and have good application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0027] Figure 1 A schematic diagram of the process flow of the bio-based polyurethane elastomer prepared in the embodiment of the present application;

[0028] Figure 2 PU prepared in the examples and comparative examples of this application PDI 5% ,PU PDI 25% ,PU PDI 40% ,PU PDI 55% ,PU PDI 70% , PU PDI 80% and PU LDI 40% Gel permeation chromatogram of

[0029] Figure 3 PU prepared in the examples and comparative examples of this application PDI 5% ,PU PDI 25% , PU PDI 40% ,PU PDI 55% ,PU PDI 70% , PU PDI 80% and PU LDI 40% Mechanical properties diagram;

[0030] Figure 4 A flow chart for recycling and reusing the bio-based polyurethane elastomer prepared in the embodiment of the present application;

[0031] Figure 5 PU prepared in the present application example PDI 40% The actual picture after 5 recycling cycles;

[0032] Figure 6PU prepared in the present application example PDI 40% "Stress-strain" diagram after 5 recycling cycles;

[0033] Figure 7 PU prepared in the present application example PDI 40% Tensile fracture strain diagram after 5 recycling cycles;

[0034] Figure 8 PU prepared in the present application example PDI 40% Tensile fracture stress diagram after 5 recycling cycles;

[0035] Fig. 9 PU prepared in the present application example PDI 40% Schematic diagram of the carrying capacity after 5 recycling cycles. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0037] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0038] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0039] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0040] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0041] It should be noted that all raw materials and reagents in the examples of the present application are purchased on the market or prepared according to conventional methods known to those skilled in the art. For example, 1,5-pentanediisocyanate (PDI), lysine diisocyanate (LDI) and 1,3-propylene glycol (PDO) are all purchased on the market.

[0042] In a first aspect, the present invention provides a bio-based polyurethane elastomer, which is prepared by addition polymerization of raw materials comprising the following components:

[0043] 45-75 parts by weight of bio-based polyol;

[0044] 22-47 parts by mass of 1,5-pentanediisocyanate;

[0045] 3-8 parts by mass of 1,3-propylene glycol;

[0046] The bio-based polyol is bio-based 1,4-butanediol or A polyol;

[0047] The A polyol is prepared by esterification and polycondensation of 1,3-propylene glycol and a dibasic acid;

[0048] The total mass of the 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 25-55% of the total mass of the raw materials.

[0049] Among them, on the one hand, it can effectively regulate the microphase separation structure of the hard segment and the soft segment, so that the bio-based polyurethane elastomer has excellent elasticity and toughness while having excellent mechanical properties and stability; on the other hand, the bio-based polyurethane elastomer prepared in this application can be regenerated after simple treatment, and after 5 recycling cycles, it can still maintain excellent load-bearing capacity and initial mechanical properties, and has good environmental friendliness; in addition, the raw materials are renewable bio-based materials, which are low in cost, can be mass-produced, and have good application value.

[0050] In the embodiment of the present application, the mass of 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 40% of the total mass of the raw materials. By limiting the content of 1,5-pentanediisocyanate and 1,3-propylene glycol, the bio-based polyurethane has excellent mechanical properties and stability, and the performance is optimal when the mass of 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 40% of the total mass of the raw materials.

[0051] In the embodiment of the present application, the bio-based polyol is preferably bio-based 1,4-butanediol or A polyol. The A polyol is prepared by a method comprising the following steps: 1,3-propylene glycol, a dibasic acid and tetrabutyl titanate are mixed for esterification reaction, and the temperature is increased for polycondensation reaction to obtain A polyol; the molecular weight of the A polyol is preferably 80,000-100,000 g / mol.

[0052] It should be noted that the specific preferred synthesis steps of the A polyol are as follows:

[0053] (1) Esterification reaction: Weigh a certain molar ratio of 1,3-propylene glycol, sebacic acid, and tetrabutyl titanate into a three-necked flask, slowly heat it from 160°C to 210°C in a N2 atmosphere, and start the stirring device after the system is melted. When the first drop of distillate appears in the water separator, it indicates that the esterification reaction has begun. Keep the reaction to produce distillate continuously and stably. When the reaction system changes from turbid to clear and no water is left in the system, the esterification reaction ends, the reaction system gradually cools down, and then enters the polycondensation stage.

[0054] (2) Condensation reaction: Before entering the high vacuum polycondensation reaction stage, low vacuum pre-condensation is required. The esterification product is first reacted at 210 °C for 1 h. After the pre-condensation stage reaction is completed, the high vacuum polycondensation reaction begins. At the same time, the reaction temperature is slowly increased from 210 °C to 240 °C for 5 h. After the reaction is completed, polyol A is obtained.

[0055] It should be noted that polyurethane refers to a polymer material containing a large number of repeating carbamate (-NHCOO-) units in the molecular chain, usually formed by the reaction of isocyanate-NCO and hydroxyl-OH. Polyurethane elastomer refers to a polymer with a glass transition temperature (T g ) is a polyurethane material below room temperature. The raw materials for producing polyurethane elastomers include bio-based polyols, 1,3-propylene glycol and 1,5-pentanediisocyanate. Among them, bio-based polyols constitute the soft segment of polyurethane elastomers due to their flexibility, and 1,3-propylene glycol and 1,5-pentanediisocyanate constitute the hard segment of polyurethane elastomers. Due to thermodynamic incompatibility, the soft and hard segments in polyurethane elastomers form a separated structure at the microscopic scale (tens to hundreds of nanometers), that is, microphase separation. At the same time, there are a large number of hydrogen bonds between polyurethane elastomer molecules, especially between carbamates and carbamates in the hard segment. This microphase separation and the large number of hydrogen bonds between molecules give polyurethane elastomers better performance than other elastomers.

[0056] In a second aspect, the present application also provides a method for preparing the bio-based polyurethane elastomer according to the first aspect, the preparation method comprising:

[0057] The bio-based polyol and 1,5-pentanediisocyanate are reacted to generate a prepolymer, and then 1,3-propylene glycol is added to carry out a vulcanization reaction to obtain the bio-based polyurethane elastomer.

[0058] In the embodiment of the present application, the temperature of the vulcanization reaction is preferably 60-90°C, and the time of the vulcanization reaction is preferably 2-4 hours. By controlling the temperature and time of the vulcanization reaction, the degree of addition polymerization can be controlled to form a uniform and stable network structure, giving the bio-based polyurethane elastomer excellent mechanical properties.

[0059] The third aspect of the present application provides the use of the bio-based polyurethane elastomer described in the first aspect or the bio-based polyurethane elastomer prepared by the preparation method described in the second aspect in building materials, public facilities, medical facilities and medical devices, and textile materials. Among them, the bio-based polyurethane elastomer prepared based on the above has excellent mechanical strength, strength, hardness and stability. After 5 recycling cycles, it still maintains excellent load bearing capacity and initial mechanical properties, and can reduce production costs, giving the finished product product competitiveness, and has broad market application prospects.

[0060] The technical solution of the present application will be further described below in conjunction with specific embodiments.

[0061] Example 1

[0062] This embodiment provides A1-biobased polyurethane elastomer (PU PDI 40% ), specifically comprising:

[0063] according to Figure 1 Preparation flow chart:

[0064] Preparation of polyol A: Weigh 1,3-propylene glycol, sebacic acid, and tetrabutyl titanate in a three-necked flask, slowly heat from 160 °C to 210 °C in a N2 atmosphere, and after the system is melted, start the stirring device, and the esterification product is reacted at 210 °C for 1 h. After the pre-polycondensation stage reaction is completed, start the high vacuum polycondensation reaction, and at the same time, slowly increase the reaction temperature from 210 °C to 240 °C for 5 h. After the reaction is completed, polyol A is obtained.

[0065] 45 g of A polyol and 25 g of 1,5-pentanediisocyanate were reacted at 60 °C for 2 h to form a prepolymer, and then 5 g of 1,3-propylene glycol was added for vulcanization reaction. The reaction was continued for 1 h. After the reaction was completed, the mixture was degassed and cooled to obtain A1-biobased polyurethane elastomer (PU PDI 40% ).

[0066] Example 2

[0067] A2-biobased polyurethane elastomer (PU) prepared in this embodiment PDI 25% ) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the raw materials used in this example are 75 g A polyol, 22 g 1,5-pentanediisocyanate and 3 g 1,3-propylene glycol to prepare A2-biobased polyurethane elastomer (PU PDI 25% ).

[0068] Example 3

[0069] A3-biobased polyurethane elastomer (PU) prepared in the present embodiment PDI 55% ) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the preparation materials in this example use 45 g A polyol, 47 g 1,5-pentanediisocyanate and 8 g 1,3-propylene glycol to prepare A3-bio-based polyurethane elastomer (PU PDI 55% ).

[0070] Example 4

[0071] This embodiment provides A4-biobased polyurethane elastomer (PU 40% ), specifically comprising:

[0072] 45 g of bio-based 1,4-butanediol and 25 g of 1,5-pentanediisocyanate were reacted at 90 °C for 2 h to form a prepolymer, and then 5 g of 1,3-propylene glycol was added for vulcanization reaction. The reaction was continued for 2 h. After the reaction was completed, the prepolymer was degassed and cooled to obtain A4-bio-based polyurethane elastomer (A1-PU 40% ).

[0073] At the same time, in order to verify the comprehensive performance of the bio-based polyurethane elastomer prepared in the above examples, the present application provides the following comparative examples for detailed description.

[0074] Comparative Example 1

[0075] B1-bio-based polyurethane elastomer (PU PDI 5% ) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the raw materials used in this comparative example are 95 g of A polyol, 3 g of 1,5-pentanediisocyanate and 2 g of 1,3-propylene glycol to prepare B1-bio-based polyurethane elastomer (PU PDI 5% ).

[0076] Comparative Example 2

[0077] B2-biobased polyurethane elastomer (PU PDI 70%) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the preparation materials in this comparative example use 30 g of A polyol, 50 g of 1,5-pentanediisocyanate and 20 g of 1,3-propylene glycol to prepare B2-bio-based polyurethane elastomer (PU PDI 70% ).

[0078] Comparative Example 3

[0079] B3-bio-based polyurethane elastomer (PU PDI 80% ) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the preparation materials in this comparative example use 20 g of A polyol, 50 g of 1,5-pentanediisocyanate and 30 g of 1,3-propylene glycol to prepare B3-bio-based polyurethane elastomer (PU PDI 80% ).

[0080] Comparative Example 4

[0081] B4-biobased polyurethane elastomer (PU LDI 40% ) The component ratio, preparation operation and process parameters are basically the same as those in Example 1, except that the preparation materials in this comparative example use 45 g of A polyol, 25 g of lysine diisocyanate and 5 g of 1,3-propylene glycol to prepare B4-bio-based polyurethane elastomer (PU LDI 40% ).

[0082] The difference between Comparative Example 4 of the present application and Example 1 is that different isocyanates are used.

[0083] The bio-based polyurethane elastomer prepared in this application is named PU PDI / LDI x% , where 1,5-pentane diisocyanate is denoted as PDI, lysine diisocyanate is denoted as LDI, PDI / LDI represents whether the hard segment in the polyurethane elastomer is PDI or LDI, and x% represents the weight percentage of the hard segment in the bio-based polyurethane elastomer.

[0084] In order to verify the molecular structure of the bio-based polyurethane elastomer prepared in the examples of the present application, the bio-based polyurethane elastomer prepared in the examples was subjected to gel permeation chromatography (GPC) test, and the results were as follows: Figure 2 As shown; among them, Figure 2 PU PDI 5% , PU PDI 25% , PU PDI 40% , PU PDI 55% , PU PDI 70% , PU PDI 80% and PU LDI 40% Gel permeation chromatogram of .

[0085] according to Figure 2 As known, the PU prepared in this application PDI 5% , PU PDI 25% , PU PDI 40% , PU PDI 55% , PU PDI70% , PU PDI 80% and PU LDI 40% The weight average molecular weight (M w ) were 95 kg / mol, 102 kg / mol, 106 kg / mol, 111 kg / mol, 107 kg / mol, 94 kg / mol and 97 kg / mol respectively; the polydispersity coefficients were 3.87, 4.23, 4.01, 4.15, 3.93, 4.85 and 3.79 respectively. These GPC results prove that we have successfully synthesized PU PDI 5% , PU PDI 25% , PU PDI 40% , PU PDI 55% , PU PDI 70% , PU PDI 80% and PU LDI 40% The weight average molecular weight and polydispersity coefficient of these 7 bio-based polyurethane elastomers meet the use requirements by strictly controlling the feed ratio of 1,5-pentanediisocyanate and 1,3-propylene glycol, lysine diisocyanate and 1,3-propylene glycol. In addition, the molecular weight and PDI of these 7 polyurethane elastomers are very similar, eliminating the influence of molecular weight and PDI on the final performance of polyurethane elastomers.

[0086] In order to verify the mechanical properties of the bio-based polyurethane elastomer prepared in the examples of this application, the bio-based polyurethane elastomer prepared in the examples was subjected to "stress-strain" and recycling tests, and the results were Figure 3 As shown; among them, Figure 3 PU PDI 5% , PU PDI 25% , PU PDI 40% , PU PDI 55% , PU PDI 70% , PU PDI 80% and PU LDI 40%Mechanical properties diagram. The mechanical properties tests of this application are all carried out in accordance with relevant national standards. After hot pressing above the melting temperature on a heating program hot stage, the tensile and bending standard specimens are obtained. Hardness: GB / T 531.2-2009; tensile strength, elongation at break, Young's modulus, toughness: GB / T 528-2009; tear strength: GB / T 529-2008; tensile elastic recovery rate: FZ 70006-2004-T. The test specimens for hardness, tensile strength, elongation at break, Young's modulus, toughness and tensile elastic recovery rate are sized: 12 mm×2 mm×1 mm. The tear strength test specimen is sized: 105 mm×15 mm×2 mm.

[0087] according to Figure 3 As far as we know, only the PU prepared in the present embodiment PDI 25% PU PDI 40% PU PDI 55% That is, when the hard segment content is 25 wt.% to 55 wt.% and the hard segment is a pure linear structure, the bio-based polyurethane elastomer will exhibit good mechanical properties.

[0088] The mechanical properties of the bio-based polyurethane elastomers prepared in the examples and comparative examples are summarized, and the test results are shown in Table 1:

[0089] Table 1 Comprehensive test results of bio-based polyurethane elastomers prepared in Examples and Comparative Examples

[0090]

[0091] According to Table 1, the PU prepared in Example 1 of the present application PDI 40% Bio-based polyurethane elastomers have optimal mechanical properties.

[0092] In order to comprehensively evaluate the recyclability of bio-based polyurethane elastomers, this application selected PU PDI 40% A detailed test was conducted for the representative, and the results were Figures 4 to 9 As shown; among them, Figure 4 A flow chart for the recycling and reuse of bio-based polyurethane elastomers; Figure 5 PU PDI 40% Recycling diagram; Figure 6 PU PDI 40% "Stress-strain" diagram after 5 recycling cycles; Figure 7 PU PDI 40% Tensile fracture strain diagram after 5 recycling cycles; Figure 8 PU PDI 40% Tensile fracture stress diagram after 5 recycling cycles; Fig. 9 PU PDI 40% Schematic diagram of the carrying capacity after 5 recycling cycles.

[0093] according to Figure 4 As is known, the bio-based polyurethane elastomer is recycled and shredded, heat treated at a temperature of 140°C to 220°C, hot pressed into film, demolded after cooling, and hot pressed into film again. When it is recycled again, the cycle is repeated and the recycling cycle operation can be carried out in sequence according to the process.

[0094] according to Figure 5-9 It can be seen that this application uses PU PDI 40% To evaluate the recyclability and recycling performance, detailed tests were conducted. Figure 5 PU is shown in PDI 40% After 5 cycles, its appearance did not change significantly. Figure 6-8 Showing PU PDI 40% Performance after 5 recycling cycles. Initially prepared PU PDI 40% The samples exhibited excellent mechanical properties, and their stress-strain curves showed high tensile strength and good ductility. After 5 recycling cycles, the stress-strain curves of the samples showed almost no significant changes, indicating that their mechanical properties remained stable. Specifically, Figure 7 and Figure 8 It shows that the mechanical properties of the initial samples and the recycled samples after 5 recyclings are basically the same, with the elongations at break being 1590±36%, 1537±28%, 1577±40%, 1593±45%, 1591±32% and 1535±32% respectively; and the tensile stresses at break being 34±3 MPa, 35±5 MPa, 36±4 MPa, 34±2 MPa, 34±3 MPa and 33±3 MPa respectively. Fig. 9 Take 0.2 g of PU after the fifth recovery PDI 40% The bottom of the machine can withstand the load of 5 kg dumbbells. Further load tests have proved that the recycled PU PDI 40% The sample was able to withstand a 5 kg dumbbell load without significant permanent deformation or damage. This fully demonstrates that PU PDI 40% After 5 recycling cycles, it still has good load-bearing capacity and structural stability.

[0095] Therefore, the bio-based polyurethane elastomer provided in the present application is obtained by the addition polymerization reaction of bio-based polyols, 1,3-propylene glycol and 1,5-pentanediisocyanate. By limiting the content of 1,5-pentanediisocyanate and 1,3-propylene glycol, the strength, mechanical properties and stability of the bio-based polyurethane can be effectively improved. At the same time, it can be regenerated after simple treatment, and after 5 recycling cycles, it can still maintain excellent load-bearing capacity and initial mechanical properties, showing excellent recyclable and reusable performance and improving resource utilization efficiency. In addition, the raw materials are renewable bio-based materials, which are low in cost and can be mass-produced, and have good application value.

[0096] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

Claims

1. A bio-based polyurethane elastomer, characterized in that: It is prepared by addition polymerization of raw materials comprising the following ingredients: 45-75 parts by weight of bio-based polyol; 22-47 parts by mass of 1,5-pentanediisocyanate; 3-8 parts by mass of 1,3-propylene glycol; The bio-based polyol is bio-based 1,4-butanediol or A polyol; The A polyol is prepared by esterification and polycondensation of 1,3-propylene glycol and a dibasic acid; The total mass of the 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 25-55% of the total mass of the raw materials.

2. The bio-based polyurethane elastomer according to claim 1, characterized in that The total mass of the 1,5-pentanediisocyanate and 1,3-propylene glycol accounts for 40% of the total mass of the raw materials.

3. The bio-based polyurethane elastomer according to claim 1 or 2, characterized in that: The A polyol is prepared by a method comprising the following steps: 1,3-propylene glycol, dibasic acid and tetrabutyl titanate are mixed for esterification reaction, and the temperature is raised for polycondensation reaction to obtain polyol A; The molecular weight of the A polyol is 80,000-100,000 g / mol.

4. The bio-based polyurethane elastomer according to claim 3, characterized in that The dibasic acid is one of sebacic acid, adipic acid and dodecanedioic acid.

5. A method for preparing a bio-based polyurethane elastomer according to any one of claims 1 to 4, characterized in that: The preparation method comprises: The bio-based polyol and 1,5-pentanediisocyanate are reacted to generate a prepolymer, and then 1,3-propylene glycol is added to carry out a vulcanization reaction to obtain the bio-based polyurethane elastomer.

6. The method for preparing a bio-based polyurethane elastomer according to claim 5, characterized in that: The temperature of the vulcanization reaction is 60-90°C.

7. The method for preparing a bio-based polyurethane elastomer according to claim 5, characterized in that: The vulcanization reaction time is 2-4 h.

8. Use of the bio-based polyurethane elastomer according to any one of claims 1 to 4 or the bio-based polyurethane elastomer prepared by the preparation method according to any one of claims 5 to 7 in building materials, automotive parts, medical supplies and textile materials.

Citation Information

Patent Citations

  • Thermoplastic polyurethane with reduced tendency to bloom from a bio-based glycol

    CN103608372A

  • Biology base polyester polyol well as preparation method and application thereof

    CN103694458A

  • Biological-type thermoplastic polyurethane elastomer and preparation method thereof

    CN109438653A

  • Thermoplastic and elastomeric polyurethanes produced from bio-based 1, 5-pentamethylene diisocyanates

    CN115322330A

  • THERMOPLASTIC POLYURETHANE COMPOSITION HAVING HIGH MECHANICAL MECHANISM, Good

    CN115702183A