Thienyl nylon as well as preparation method and application thereof
By synthesizing thiophene-based nylon at low temperatures, the problems of dependence on petroleum and safety risks of high temperature and high pressure in traditional nylon production have been solved, providing high-performance bio-based nylon materials suitable for a variety of applications.
Patent Information
- Application Number
- CN202310582492.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional nylon production relies on non-renewable petroleum resources. The high-temperature and high-pressure reaction poses safety risks and is costly. Furthermore, the material has a simple structure and insufficient performance, making it difficult to meet the diverse needs of industries.
Thiophene-based nylon was synthesized at low temperature under nitrogen or argon protection by adding organic solvents and catalysts. The nylon was then copolymerized with diacid and diamine monomers to prepare a novel nylon material with bio-based characteristics.
It has achieved low-cost and safe nylon synthesis, expanded the range of material applications, improved material performance, and possesses high mechanical strength and toughness, making it suitable for high-temperature environments.
Smart Images

Figure CN119019679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of new polymer materials, and in particular to thienyl nylon and a preparation method and application thereof. Background Art
[0002] Nylon has excellent comprehensive properties and is the most widely used engineering plastic. According to the chemical structure of the nylon main chain, nylon can be divided into three categories: aromatic, aliphatic and semi-aromatic. Nylon is strong and wear-resistant, has low density, is light, has good elasticity, is fatigue-resistant, and has good chemical stability. It is widely used in textiles, machinery, electrical, chemical, automotive, daily chemicals, medicine, and construction. Aliphatic nylon includes nylon 66 and nylon 56; aromatic nylon mainly includes poly(m-phenylene isophthalamide) and poly(p-phenylene terephthalamide).
[0003] With the development of social industry, the demand for nylon compounds is growing rapidly. However, the main raw material for traditional nylon production is non-renewable resources - petroleum. With the continuous reduction of petroleum resources and people's increasing attention to environmental issues, in the context of carbon emission reduction, the development of bio-based polymer materials is the main research direction to replace traditional petroleum-based materials. At the same time, in practical applications, traditional nylon materials still have disadvantages such as single structure, few types, and insufficient performance, which cannot meet the needs of the industry. Therefore, it is urgent to develop new bio-based high-performance nylon materials.
[0004] 2,5-Thiophenedicarboxylic acid is an important biomass platform compound that can be prepared from biomass raw materials such as natural agricultural and forestry plants. The raw material source is green and low-priced, and can effectively reduce carbon dioxide emissions. 2,5-Thiophenedicarboxylic acid is the core monomer raw material of thienyl nylon, and the synthesized nylon material has the characteristics of green and environmental protection.
[0005] Therefore, the development of thiophene nylon materials can, on the one hand, help solve the defects of nylon materials such as single structure, few product types, and insufficient performance. It can effectively promote the diversification of bio-based polymer materials and fill the gap in the application of thiophene nylon materials. On the other hand, it can overcome the environmental pollution problems caused by traditional petroleum-based and benzene-based polymer materials, which is conducive to reducing the use of petroleum resources, helping to reduce carbon emissions and achieve sustainable development of the polymer materials industry.
[0006] 202110224040.4 discloses a high-temperature resistant nylon and a synthesis method thereof, which involves the synthesis of semi-aromatic thiophene nylon, but does not study thiophene-based fully aromatic nylon. The reaction requires a certain pressure and high temperature, and the reaction temperature is between 230 and 350°C.
[0007] At present, the industrial production of benzene semi-aromatic nylon mainly adopts the high temperature and high pressure solution polycondensation method. CN201410181117.4, CN201110360514.4 and others all adopt this method. High temperature and high pressure have very high requirements on the reactor. This type of equipment is relatively expensive and has higher safety risks. There is a risk of explosion and deflagration, a long reaction time and high production cost. Summary of the invention
[0008] One object of the present invention is to disclose a thienyl nylon; another object of the present invention is to provide a method for preparing thienyl nylon, which has a mild reaction process, does not require high temperature and high pressure, is simple to operate, and has low production cost; another object of the present invention is to provide an application of thienyl nylon.
[0009] The purpose of the present invention can be achieved through the following technical solutions:
[0010] A thienyl nylon, wherein the polymer is derived from a diacid monomer and a diamine monomer, wherein the diacid monomer is a copolymer of thiophene dicarboxylic acid or its derivatives, or a copolymer of thiophene dicarboxylic acid or its derivatives and an aromatic diacid, an aliphatic diacid, or a heterocyclic diacid; and the diamine monomer is an aromatic diamine, an aliphatic diamine, a heterocyclic diamine, or a copolymer of an aromatic diamine and an aliphatic diamine.
[0011] In the technical solution of the present invention, the thienyl nylon comprises a repeating unit having a chemical structure shown in Formula I:
[0012]
[0013] wherein R1 is selected from -CH3, -C2H5, or C3-C 25 A straight chain, branched or cyclic alkane, wherein the heteroatom is selected from O, N, Si and S; or R1 is selected from -Cl, -Br, -F, -I, -OH, -NH2 and -SH.
[0014] wherein R2 is selected from -CH3, -C2H5, or C3-C 25 A straight chain, branched or cyclic alkane, wherein the heteroatom is selected from O, N, Si and S; or R2 is selected from -Cl, -Br, -F, -I, -OH, -NH2 and -SH.
[0015] In some specific technical solutions, the thienyl nylon has the following structural formula (II):
[0016]
[0017] N≥2; X, Y are selected from substituted or unsubstituted benzene ring, heterocycle, alkane.
[0018] In some specific technical solutions, the thiophene dicarboxylic acid is 2,5-thiophene dicarboxylic acid; 2,4-thiophene dicarboxylic acid; 3,4-thiophene dicarboxylic acid or 2,3-thiophene dicarboxylic acid, and the derivative of the thiophene dicarboxylic acid is thiophene dicarboxylic acid chloride.
[0019] In some specific technical schemes, the diacid monomer further comprises a diacid comonomer and its derivatives, wherein the comonomer is selected from one or more of terephthaloyl chloride, isophthaloyl chloride, 2,6-pyridine dicarboxylic acid chloride, 1,3,5-benzene trimeroyl chloride, phthaloyl chloride, 1,9-naphthalene dicarboxylic acid chloride, 2,6-pyridine dicarboxylic acid chloride, 2,5-furan dicarboxylic acid chloride, 2,5-pyrazine dicarboxylic acid chloride, 4,4-chloroformylphenyl ether, 1,4-cyclohexane dicarboxylic acid chloride, 2,5-pyrrole dicarboxylic acid chloride, succinyl chloride, glutaryl chloride, adipoyl chloride, azelaic acid chloride, fumaric acid and malic acid;
[0020] The diamine copolymer monomers include: m-phenylenediamine, naphthalene diamine, p-phenylenediamine, 2,5-pyridinediamine, 4,4-diaminodiphenyl ether, 3,4-diaminodiphenyl ether, 4,4-diaminodiphenyl sulfone, 3,3-diaminodiphenyl sulfone, 1,4-bis(4-aminophenoxy)benzene, butanediamine, pentamethylenediamine, hexamethylenediamine, 3,3'-dimethylbenzidine; 2,6-naphthalene diamine and mixtures thereof, and heteroatom-substituted diamines of the above diamine monomers; preferably, the heteroatom is F, Cl, Br, I, N, O, S, P, OH or NH2.
[0021] In some more preferred technical solutions: the diacid monomer is a mixture of 2,5-thiophene dicarboxylic acid chloride and isophthaloyl chloride in a mass ratio of 1 to 3:1 to 3; or the diacid monomer is thiophene dicarboxylic acid chloride, or the diacid monomer is a mixture of thiophene dicarboxylic acid chloride and terephthaloyl chloride in a mass ratio of 1 to 3:1 to 3.
[0022] In some more preferred technical solutions: the diamine monomer is m-phenylenediamine, or the diamine monomer is 3,4-diaminodiphenyl ether, or the diamine monomer is p-phenylenediamine, or the diamine monomer is 4,4-diaminodiphenyl ether.
[0023] In some of the most preferred technical solutions: the combination of the diacid comonomer and the diamine comonomer is as follows:
[0024]
[0025] A method for preparing the above-mentioned thienyl nylon comprises the following steps: under the protection of nitrogen or argon, adding an organic solvent, a diamine monomer, and a catalyst in sequence, maintaining the temperature at -5°C-25°C, and adding a diacid monomer for reaction to obtain thienyl nylon.
[0026] In the above preparation method: any one of acetonitrile, tetrahydrofuran, dichloromethane, dichloroethane, pyridine, N-methylformamide, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or a mixture thereof; preferably: the weight of the organic solvent is 4-15 times that of the diacid monomer.
[0027] In the above preparation method, the catalyst is a boron catalyst, preferably: the boron catalyst is one or more of 4-(2-thiophenyl)phenylboric acid, phenylboric acid or 2-pyridineboric acid.
[0028] In the above preparation method, the molar ratio of diamine monomer to diacid monomer is 0.9-1.2:1; the molar ratio of catalyst to diacid monomer is 0.01-0.1:1.
[0029] In the technical solution of the present invention: the application of the thienyl nylon in polymer membrane materials, fiber materials and engineering plastics.
[0030] Beneficial effects of the present invention:
[0031] (1) The present invention provides a bio-based polymer material with a new structure, filling the gap in the field of thiophene-based nylon materials.
[0032] (2) The thienyl nylon prepared by the present invention has good solubility in common polar solvents, overcoming the defects of traditional aromatic nylon that is difficult to process and utilize. Therefore, the present invention broadens the application range of nylon materials.
[0033] (3) The present invention relates to a preparation method with mild reaction conditions, simple operation, short reaction time and high polymerization efficiency.
[0034] (4) Thiophene dicarboxylic acid, one of the monomers of the polymer provided by the present invention, is derived from biomass, has the characteristics of large yield and renewable nature, alleviates the pollution and energy shortage problems caused by petrochemical products, and helps to achieve the goal of "carbon emission reduction".
[0035] (5) The polymer obtained by the present invention can be prepared into film materials, high temperature resistant materials, fiber materials, and fabrics; the polymer obtained has high performance nylon. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the appearance of the film sample prepared in Example 10. DETAILED DESCRIPTION
[0037] The thienyl nylon provided by the present invention has the following general structural formula (II):
[0038]
[0039] Formula (II), where n is greater than 2
[0040] As used herein, "biobased" or "biomass" refers to compounds that are derived from agricultural and forestry plants and contain only renewable carbon, rather than fossil fuel-based or petroleum-based carbon.
[0041] Thiophene nylon may be derived from any suitable isomer of thiophene dicarboxylic acid such as 2,5-thiophene dicarboxylic acid; 2,4-thiophene dicarboxylic acid; 3,4-thiophene dicarboxylic acid; 2,3-thiophene dicarboxylic acid or derivatives thereof.
[0042] As used herein, the term "substituted or unsubstituted thiophene dicarboxylic acid or its derivatives" means that the thiophene ring may have substituents R1 and R2. When both R1 and R2 are H atoms, the thiophene dicarboxylic acid or its derivatives are unsubstituted; and when one of R1 and R2 is not H, the thiophene dicarboxylic acid or its derivatives are substituted.
[0043] In one embodiment, the thienyl nylon is a copolymer (random or block) derived from thiophene dicarboxylic acid, a diacid comonomer, and a diamine monomer. The diacid comonomer is selected from terephthaloyl chloride, isophthaloyl chloride, 2,6-pyridine dicarboxylic acid chloride, 1,3,5-benzene trimeryl chloride, phthaloyl chloride, 1,9-naphthalene dicarboxylic acid chloride, 4,4-chloroformylphenyl ether, 1,4-cyclohexane dicarboxylic acid chloride, succinyl chloride, glutaryl chloride, adipic chloride, azelaic chloride, fumaric acid, and malic acid. The molar ratio of thiophene dicarboxylic acid to the diacid comonomer can be any range, for example, the molar ratio of any component can be greater than 1:100, or alternatively, in the range of 1:100 to 100:1 or 1:9 to 9:1 or 1:3 to 3:1 or 1:1.
[0044] In another embodiment, the thienyl nylon is a copolymer (random or block) derived from thiophenedicarboxylic acid, a diamine monomer and a diamine comonomer. Metaphenylenediamine, naphthalenediamine, p-phenylenediamine, 2,5-pyridinediamine, 4,4-diaminodiphenyl ether, 3,4-diaminodiphenyl ether, 4,4-diaminodiphenyl sulfone, 3,3-diaminodiphenyl sulfone, 1,4-bis(4-aminophenoxy)benzene, pentamethylenediamine, hexamethylenediamine, 3,3'-dimethylbenzidine; 2,6-naphthalenediamine; the molar ratio of the diamine comonomers to each other can be any range, for example, the molar ratio of any component can be greater than 1:100, or alternatively, in the range of 1:100 to 100:1 or 1:9 to 9:1 or 1:3 to 3:1 or 1:1.
[0045] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0046] Example 1
[0047] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 10.8 g of m-phenylenediamine, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 10.45 g of 2,5-thiophene dicarboxylic acid chloride and 10.15 g of isophthalic acid chloride, maintain the temperature at 0°C-20°C, react for 1 hour, and obtain thiophenyl nylon compound 1. The product has an inherent viscosity of 2.52 dL / g.
[0048] Example 2
[0049] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 20.2 g of 3,4-diaminodiphenyl ether, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophenedicarboxylic acid chloride, maintain the temperature at 0°C-20°C, react for 1 hour, and obtain thiophenyl nylon compound 2. 1 H NMR (400 MHz, DMSO) δ 10.59 (s, 2H), 8.12 (m, 2H), 7.83 (m, 2H), 7.45 (m, 3H), 7.27 (m, 2H), 6.77 (m, 1H). The inherent viscosity of the product was 2.75 dL / g.
[0050] Example 3
[0051] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 10.8 g of p-phenylenediamine, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophenedicarboxylic acid chloride, maintain the temperature at 0°C-20°C, and react for 1 hour to obtain thiophenyl nylon compound 3. 1H NMR (400 MHz, DMSO) δ8.47 (s, 2H), 8.25 (s, 2H). The product logarithmic viscosity is 2.05 dL / g.
[0052] Example 4
[0053] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 108 g of m-phenylenediamine, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophenedicarboxylic acid chloride, maintain the temperature at 0°C-20°C, and react for 1 hour to obtain thiophenyl nylon compound 4. 1 H NMR (500 MHz, DMSO) δ 10.52 (m, 2H), 8.32 (s, 1H), 8.14 (s, 2H), 7.53 (m, 2H), 7.37 (m, 1H). The inherent viscosity of the product was 2.12 dL / g.
[0054] Example 5
[0055] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 20.2 g of 4,4-diaminodiphenyl ether, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophenedicarboxylic acid chloride, maintain the temperature at 0°C-20°C, and react for 1 hour to obtain thiophenyl nylon compound 5. 1 HNMR (500 MHz, DMSO) δ 10.53 (d, J = 47.9 Hz, 2H), 8.12 (d, J = 36.7 Hz, 2H), 7.79 (m, 4H), 7.01 (m, 4H). The inherent viscosity of the product is 2.63 dL / g.
[0056] Example 6
[0057] Under the protection of nitrogen or argon, 110 g of organic solvent N-methylpyrrolidone, 20.2 g of 4,4-diaminodiphenyl ether and 0.355 g of catalyst 4-(2-thienyl)phenylboronic acid were added in sequence, and the mixture was stirred. Then 10.45 g of 2,5-thiophenedicarboxylic acid chloride and 9.6 g of furanedicarboxylic acid chloride were added. The temperature was maintained at 0°C-20°C and the reaction was carried out for 1 hour to obtain thienyl nylon compound 6. 1H NMR (400 MHz, DMSO) δ10.43 (s, 1H), 10.33 (s, 1H), 8.02 (d, J=14.5 Hz, 1H), 7.76 (d, J=8.2 Hz, 4H), 7.43 (s, 1H), 7.07 (m, 4H).. The inherent viscosity of the product was 1.98 dL / g.
[0058] Example 7
[0059] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 54 g of m-phenylenediamine, 10.1 g of 4,4-diaminodiphenyl ether, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophenedicarboxylic acid chloride, maintain the temperature at 0°C-20°C, and react for 1 hour to obtain thiophenyl nylon compound 7. 1 HNMR (400MHz, DMSO) δ10.50 (m, 2H), 8.11 (dd, J = 15.9, 11.7 Hz, 2H), 7.76 (dd, J = 22.2, 8.3 Hz, 2H), 7.57 (m, 1H), 7.31 (m, 1H), 7.00 (m, 2H). The inherent viscosity of the product is 2.67 dL / g.
[0060] Example 8
[0061] Under nitrogen or argon protection, add 110g of organic solvent N-methylpyrrolidone, 5.4g of m-phenylenediamine, 5.4g of p-phenylenediamine, and 0.355g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9g of 2,5-thiophene dicarboxylic acid chloride, maintain the temperature at 0℃-20℃, react for 1 hour, and obtain thiophenyl nylon compound 8. The NMR data are as follows: 1 HNMR (400 MHz, DMSO) δ 10.55 (d, 2H), 8.32 (s, 0.5H), 8.15 (s, 0.5H), 7.76 (m, 1H), 7.52 (m, 1H), 7.36 (m, 0.5H). The inherent viscosity of the product is 2.24 dL / g.
[0062] Example 9
[0063] Under nitrogen or argon protection, add 110 g of organic solvent N-methylpyrrolidone, 24.8 g of 4,4-diaminodiphenyl sulfone, and 0.355 g of catalyst 4-(2-thiophenyl)phenylboronic acid in sequence, stir, then add 20.9 g of 2,5-thiophene dicarboxylic acid chloride, maintain the temperature at 0°C-20°C, react for 1 hour, and obtain thiophenyl nylon compound 9. The NMR data are as follows: 1 H NMR (400 MHz, DMSO) δ 10.88 (d, J = 28.5 Hz, 2H), 8.14 (s, 2H), 7.44 (m, 4H), 6.59 (m, 4H). The inherent viscosity of the product was 2.04 dL / g.
[0064] Comparative Example 1: (No catalyst was added, other operations were the same as in Example 1)
[0065] No catalyst was added, and other implementation methods were the same as in Example 1. The inherent viscosity of the product was 0.96 dL / g.
[0066] Comparative Example 2: (the catalyst was changed to sodium hypophosphite, and other operations were the same as in Example 1)
[0067] The catalyst used was 0.15 g of sodium hypophosphite, and the other implementation methods were the same as those in Example 1. The inherent viscosity of the product was 0.65 dL / g.
[0068] It can be seen from Comparative Examples 1 and 2 that the use of 4-(2-thiophenyl)phenylboronic acid as a catalyst has a higher polymerization efficiency and a higher intrinsic viscosity.
[0069] Example 10
[0070] 5g of nylon obtained in Example 3 was dissolved in 20ml of NMP and mechanically stirred at room temperature for 5h to obtain a uniform polymer solution. The obtained solution was evenly coated on a glass plate and dried at 180°C. It was placed in water and fell off to obtain a high-strength nylon film. The thermodynamic properties of the film are shown in Table 1. The prepared film samples are as follows Figure 1 :
[0071] Embodiment 11 to Embodiment 18,
[0072] The implementation method is the same as in Example 10, except that the nylon material is different, as follows:
[0073] In Example 11, the nylon material adopts thienyl nylon compound II (Example 2)
[0074] In Example 12, the nylon material adopts thienyl nylon compound 1 (Example 1)
[0075] In Example 13, the nylon material adopts thienyl nylon compound IV (Example 4)
[0076] In Example 14, the nylon material adopts thienyl nylon compound V (Example 5)
[0077] In Example 15, the nylon material adopts thienyl nylon compound VI (Example 6)
[0078] In Example 16, the nylon material is thienyl nylon compound VII (Example 7)
[0079] In Example 17, the nylon material adopts thienyl nylon compound eight (Example 8)
[0080] In Example 18, the nylon material adopts thienyl nylon compound nine (Example 9)
[0081] Comparative Example 3:
[0082] Based on Example 6, only the thiophene dicarboxylic acid chloride was replaced by terephthaloyl dichloride, and other parameters remained unchanged, and the inherent viscosity was 1.85 dL / g. The film was prepared according to Example 1.
[0083] The thermodynamic properties of the films are shown in Table 1.
[0084] Table 1
[0085]
[0086] Comparative Example 4 refers to the product prepared by Examples 1 to 6 of Patent 202110224040.4.
[0087] As shown in Table 1, the analysis of Example 15 and Comparative Example 3 shows that the mechanical properties of the material are more excellent after the introduction of the thienyl structure. The analysis of Examples 10-18 and Comparative Example 4 shows that the thienyl nylon material disclosed in the present invention has better mechanical strength, better toughness, and excellent tensile properties, and can be used under heat and high temperature conditions. It has good application potential in the field of new materials.
Claims
1. A thienyl nylon, characterized in that: The polymer is derived from a diacid monomer and a diamine monomer. The diacid monomer is: thiophene dicarboxylic acid or its derivatives, a copolymerized monomer consisting of thiophene dicarboxylic acid or its derivatives and an aromatic diacid or an aliphatic diacid or a heterocyclic diacid; the diamine monomer is: a copolymerized monomer consisting of an aromatic diamine, an aliphatic diamine, a heterocyclic diamine, or an aromatic diamine and an aliphatic diamine.
2. The thienyl nylon according to claim 1, characterized in that: The thienyl nylon comprises a repeating unit having a chemical structure shown in Formula I: wherein R1 is selected from -CH3, -C2H5, or C3-C 25 A straight chain, branched or cyclic alkane, wherein the heteroatom is selected from O, N, Si and S; or R1 is selected from -Cl, -Br, -F, -I, -OH, -NH2 and -SH. wherein R2 is selected from -CH3, -C2H5, or C3-C 25 A straight chain, branched or cyclic alkane, wherein the heteroatom is selected from O, N, Si and S; or R2 is selected from -Cl, -Br, -F, -I, -OH, -NH2 and -SH.
3. The thienyl nylon according to claim 2, characterized in that: The thienyl nylon has the following general structural formula (II): n≥2; X, Y are selected from substituted or unsubstituted benzene ring, heterocycle, alkane.
4. The thienyl nylon according to claim 1, characterized in that: The thiophene dicarboxylic acid is 2,5-thiophene dicarboxylic acid; 2,4-thiophene dicarboxylic acid; 3,4-thiophene dicarboxylic acid or 2,3-thiophene dicarboxylic acid, and the derivative of the thiophene dicarboxylic acid is thiophene dicarboxylic acid chloride.
5. The thienyl nylon according to claim 1, characterized in that: The diacid monomer further comprises a diacid comonomer and its derivatives, wherein the comonomer is selected from one or more of terephthaloyl chloride, isophthaloyl chloride, 2,6-pyridine dicarboxylic acid chloride, 1,3,5-benzene trimeroyl chloride, phthaloyl chloride, 1,9-naphthalene dicarboxylic acid chloride, 2,6-pyridine dicarboxylic acid chloride, 2,5-furan dicarboxylic acid chloride, 2,5-pyrazine dicarboxylic acid chloride, 4,4-chloroformylphenyl ether, 1,4-cyclohexane dicarboxylic acid chloride, 2,5-pyrrole dicarboxylic acid chloride, succinyl chloride, glutaryl chloride, adipoyl chloride, azelaic acid chloride, fumaric acid and malic acid; The diamine copolymer monomers include: m-phenylenediamine, naphthalene diamine, p-phenylenediamine, 2,5-pyridinediamine, 4,4-diaminodiphenyl ether, 3,4-diaminodiphenyl ether, 4,4-diaminodiphenyl sulfone, 3,3-diaminodiphenyl sulfone, 1,4-bis(4-aminophenoxy)benzene, butanediamine, pentamethylenediamine, hexamethylenediamine, 3,3'-dimethylbenzidine; 2,6-naphthalene diamine and mixtures thereof, and heteroatom-substituted diamines of the above diamine monomers; preferably, the heteroatom is F, Cl, Br, I, N, O, S, P, OH or NH2.
6. A method for preparing thienyl nylon according to claim 1, characterized in that: The method comprises the following steps: Under the protection of nitrogen or argon, an organic solvent, a diamine monomer, and a catalyst are added in sequence, the temperature is maintained at -5°C to 25°C, and a diacid monomer is added to react to obtain thienyl nylon.
7. The method for preparing thienyl nylon according to claim 6, characterized in that: The organic solvent is any one of acetonitrile, tetrahydrofuran, dichloromethane, dichloroethane, pyridine, N-methylformamide, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or a mixture thereof; preferably, the weight of the organic solvent is 4-15 times that of the diacid monomer.
8. The preparation of a thienyl nylon according to claim 6, characterized in that: The catalyst is a boron catalyst, preferably: the boron catalyst is one or more of 4-(2-thiophenyl)phenylboronic acid, phenylboronic acid or 2-pyridineboronic acid.
9. The preparation of a thienyl nylon according to claim 6, characterized in that: The molar ratio of diamine monomer to diacid monomer is 0.9-1.2:1; the molar ratio of catalyst to diacid monomer is 0.01-0.1:1; preferably, the molar ratio of catalyst to diacid monomer is 0.01-0.02:
1.
10. Use of the thienyl nylon according to claim 1 in polymer film materials, fiber materials and engineering plastics.
Citation Information
Cited By
Battery diaphragm as well as preparation method and application thereof
CN120565995A