Preparation method of zinc coordination polymer and application of zinc coordination polymer in catalysis of conversion of aryl substituted ethylene into aryl formaldehyde / aryl ketone derivative
Catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde/aryl ketone derivatives by zinc coordination polymers, the problems of complex synthesis, expensive raw materials and unfriendly environment in traditional methods are solved, and high-efficiency, low-cost and environmentally friendly catalysis is achieved. Effect.
Patent Information
- Application Number
- CN202411191715.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The traditional method of preparing aryl formaldehyde/aryl ketone derivatives has complex synthesis process, expensive initial raw materials, poor reaction selectivity, low efficiency and uneconomic environment, which limits its application.
Using a zinc coordination polymer as a catalyst, by placing trimethylolic acid, 2,4,6-tri(4-pyridyl)-1,3,5-triazine and zinc nitrate hexahydrate in methanol and N, Reacted in a mixed solution of N-dimethylacetamide, a novel zinc coordination polymer was prepared for catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde/aryl ketone derivatives.
The reaction raw materials are cheap and easy to obtain, have high selectivity, mild conditions, simple operation, and environmentally friendly catalytic effects, with high conversion rate and chemical stability, and are suitable for large-scale production.
Smart Images

Figure CN119019703A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a preparation method of a zinc coordination polymer and application of the zinc coordination polymer in catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives. Background Art
[0002] Aryl formaldehyde / aryl ketone derivatives are a class of commonly used chemical raw materials and important organic synthesis intermediates. Traditional methods for preparing aryl formaldehyde include hydrolysis of chloroarene, toluene oxidation, aryl methanol oxidation, aryl formic acid hydrogenation reduction and indirect electrooxidation. However, these methods have many shortcomings, such as complex synthesis process, expensive initial raw materials, poor reaction selectivity and low efficiency, the reaction needs to be carried out under inert gas protection and is not environmentally friendly, which limits the further application of aryl formaldehyde / aryl ketone derivatives.
[0003] Therefore, developing a method with cheap and readily available reaction raw materials, high reaction selectivity, mild reaction conditions and environmental friendliness will have important research significance and application value. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a preparation method of a zinc coordination polymer and its application in catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives. The present invention provides a novel zinc coordination polymer, which can be used as a catalyst to selectively catalyze the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives. The method of the novel zinc coordination polymer as a catalyst to selectively catalyze the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives has the characteristics of cheap and readily available reaction raw materials, high reaction selectivity, mild reaction conditions, easy operation and environmental friendliness.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention:
[0007] A method for preparing a zinc coordination polymer comprises the following steps:
[0008] Trimesic acid, 2,4,6-tris(4-pyridyl)-1,3,5-triazine and zinc nitrate hexahydrate are dissolved in a mixed solution of methanol and N,N-dimethylacetamide, and stirred evenly to obtain a solution. The solution is heated at 90-110° C. and cooled to room temperature to obtain light yellow crystals, which are the zinc coordination polymer.
[0009] Preferably, in the preparation method of the zinc coordination polymer, the trimesic acid 2,4,6-Tris(4-pyridyl)-1,3,5-triazine The molar ratio of zinc nitrate hexahydrate is 1:1:2.
[0010] Preferably, in the method for preparing the zinc coordination polymer, the volume ratio of methanol to N,N-dimethylacetamide is 1:(3-3.5).
[0011] Preferably, in the method for preparing the zinc coordination polymer, the heating time is 48 to 72 hours, and the cooling rate during the cooling is 10 to 15° C. / min.
[0012] The second technical solution of the present invention:
[0013] The invention also provides a zinc coordination polymer prepared by the method.
[0014] The zinc coordination polymer provided by the invention can be used as a green catalyst to directly convert aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives.
[0015] The third technical solution of the present invention:
[0016] The invention also provides the use of the zinc coordination polymer in catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives (aromatic formaldehyde or aromatic ketone derivatives).
[0017] In the above application of the present invention, the aromatic substituted ethylene includes styrene and its derivatives.
[0018] The fourth technical solution of the present invention:
[0019] The present invention also provides a method for catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives, comprising dissolving aromatic substituted ethylene in ethanol, then adding the zinc coordination polymer and hydrogen peroxide, heating the obtained mixed solution to 60° C., adding ethyl acetate for extraction after the raw material (i.e. aromatic substituted ethylene) has reacted completely, and draining the solvent to obtain a crude product; and separating the crude product by column chromatography to obtain the aromatic formaldehyde / aromatic ketone derivative.
[0020] Preferably, in the method for catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives, the amount of zinc coordination polymer added is 0.1 mol% of aromatic substituted ethylene, such as when the amount of aromatic substituted ethylene added is 1 mol, the amount of zinc coordination polymer added is 0.001 mol.
[0021] Preferably, in the method for catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives, the reaction time is 6 to 12 hours.
[0022] Preferably, in the method for catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives, the molar ratio of the aromatic substituted ethylene to the hydrogen peroxide is 1:3, and the mass fraction of the hydrogen peroxide is 30%.
[0023] Preferably, in the method for catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives, the eluent is petroleum ether and ethyl acetate, the volume ratio of petroleum ether to ethyl acetate is 1:0 to 20:1, and the volume of ethyl acetate is not 0.
[0024] More preferably, the general structural formula of the aryl-substituted ethylene is Where R 1 =H, 4-OMe, 4-Br or 4-F, R 2 =Ph or H, the reaction route to generate aromatic formaldehyde or aromatic ketone products is as follows:
[0025]
[0026] In the method of catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives of the present invention, the yield of aryl formaldehyde / aryl ketone derivatives is 91-97%.
[0027] Compared with the prior art, the present invention has the following advantages and technical effects:
[0028] (1) The method of the present invention has low requirements for synthesis equipment, is simple and convenient to operate, has readily available raw materials, is low in cost, has mild reaction conditions, can be mass-produced, and has a high yield and good purity of the prepared zinc coordination polymer material.
[0029] (2) The zinc coordination polymer prepared by the present invention has good chemical stability and thermal stability, can stably exist in an aqueous solution with a pH of 2-12 for 24 hours, and has a heat resistance of up to 300°C.
[0030] (3) The zinc coordination polymer prepared by the present invention has the characteristics of high conversion rate and high chemical stability as a catalyst, and has extremely high catalytic activity for the reaction of converting aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives. In addition, the dosage is low (only 0.1 mol%), the catalytic reaction conditions are mild, and the operation is easy, so the catalyst has good practical value and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0032] Figure 1 This is an X-ray single crystal structure diagram of the zinc coordination polymer prepared in Example 1 of the present invention;
[0033] Figure 2 The three-dimensional structure diagram of the zinc coordination polymer prepared in Example 1 of the present invention;
[0034] Figure 3 This is a thermogravimetric curve of the zinc coordination polymer obtained in Example 1 of the present invention;
[0035] Figure 4 The XRD pattern of the zinc coordination polymer obtained in Example 1 of the present invention;
[0036] Figure 5 The XRD patterns of the zinc coordination polymer obtained in Example 1 of the present invention after being immersed in aqueous solutions with pH values of 2 and 12 for 24 hours;
[0037] Figure 6 This is a thermogravimetric curve of the zinc coordination polymer obtained in Example 2 of the present invention;
[0038] Figure 7 The XRD pattern of the zinc coordination polymer obtained in Example 2 of the present invention;
[0039] Figure 8 This is a graph of the catalytic yield of the zinc coordination polymer prepared in Example 2 of the present invention catalyzing the conversion of styrene into benzaldehyde and recycling it;
[0040] Fig. 9 This is the XRD pattern of the zinc coordination polymer prepared in Example 2 of the present invention catalyzing the conversion of styrene into benzaldehyde before and after recycling. DETAILED DESCRIPTION
[0041] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0042] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0043] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0044] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0045] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0046] All raw materials used in the examples of the present invention are commercially available.
[0047] In the embodiments of the present invention, trimesic acid, 2,4,6-tris(4-pyridyl)-1,3,5-triazine, zinc nitrate hexahydrate, methanol and N,N-dimethylacetamide are all analytically pure. Aryl-substituted ethylene and hydrogen peroxide (the mass fraction of hydrogen peroxide is 30%) are all analytically pure. Ethanol, petroleum ether and ethyl acetate are all analytically pure.
[0048] In the embodiments of the present invention, unless otherwise specified, the room temperature is 25±2°C.
[0049] The technical solution of the present invention is further illustrated by the following embodiments.
[0050] Example 1
[0051] A method for preparing a zinc coordination polymer:
[0052] 0.1mmol of trimesic acid, 0.1mmol of 2,4,6-tris(4-pyridyl)-1,3,5-triazine and 0.2mmol of zinc nitrate hexahydrate were added to a mixed solution containing 1mL of methanol and 3mL of N,N-dimethylacetamide, stirred for 5 minutes under air atmosphere at room temperature, and then the stirred solution was transferred to a 15mL Teflon autoclave, heated to 100°C in an oven and kept constant for 48 hours, and after the reaction was completed, the temperature was lowered to room temperature at a rate of 10°C / h to obtain pale yellow crystals, which were filtered, washed with methanol and vacuum dried for 2 hours to obtain a zinc coordination polymer with a yield of 72%. The synthesized zinc coordination polymer was ground through a 100-mesh sieve and set aside.
[0053] The X-ray single crystal structure of the zinc coordination polymer prepared in this example is shown in Figure 1 , the three-dimensional structure diagram is shown in Figure 2 .from Figure 1 and Figure 2 It can be seen that each zinc atom coordinates with two carboxyl groups of trimesic acid and two pyridine nitrogen atoms of 2,4,6-tris(4-pyridyl)-1,3,5-triazine to form a tetrahedral configuration; then the carboxyl group of trimesic acid and the pyridine nitrogen atom of 2,4,6-tris(4-pyridyl)-1,3,5-triazine both coordinate with the zinc atom to form a three-dimensional coordination polymer.
[0054] The thermal stability of the zinc coordination polymer product prepared in this example was characterized by a thermogravimetric analysis experiment. Specifically, the temperature was raised at a heating rate of 10°C / min under nitrogen purge to measure the thermal gravimetric curve of the zinc coordination polymer. The results are shown in Figure 3 It can be seen that there is a weight loss of about 15% in the temperature range from room temperature to 140°C, indicating that the zinc coordination polymer product contains more solvent molecules. After the solvent molecules evaporate, the zinc coordination polymer product has basically no weight loss at 140-350°C, indicating that the zinc coordination polymer product can exist stably in this temperature range and has good thermal stability. In the range of 350-800°C, the zinc coordination polymer product loses weight sharply, indicating that the zinc coordination polymer product begins to decompose.
[0055] The zinc coordination polymer prepared in this example was subjected to XRD analysis, and the results are shown in Figure 4 It can be seen that the characteristic peaks of the XRD spectrum of powder diffraction are consistent with the characteristic peaks of theoretical simulation, indicating that the structure of the synthesized zinc coordination polymer is consistent with the simulated structure and is a pure phase.
[0056] The chemical stability of the zinc coordination polymer prepared in this example was analyzed, and the results are shown in Figure 5It can be seen that after the zinc coordination polymer prepared in this example was immersed in acidic and alkaline aqueous solutions with pH values of 2 and 12 respectively for 24 hours, its XRD spectrum was consistent with the theoretical simulation spectrum. Figure 1 This indicates that the structure of the coordination polymer does not change in acidic and alkaline aqueous solutions with pH values of 2 and 12, respectively, and it has good chemical stability.
[0057] The X-ray single crystal diffraction data of the coordination polymer prepared in this example are shown in Table 1.
[0058] Table 1 X-ray single crystal diffraction data of zinc coordination polymers
[0059]
[0060]
[0061] Effect Example 1 (Taking the zinc coordination polymer prepared in Example 1 as an example)
[0062] Catalytic aryl substitution of ethylene to synthesize aryl formaldehyde / aryl ketone derivatives 2a~2f:
[0063] (1) Synthesis of compound 2a
[0064] 0.001 mol of styrene 1a Dissolve in 2 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.003 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 8 hours, and wait for the reaction of raw material 1a to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2a The yield was 91%. NMR spectrum data of compound 2a: 1 H NMR (400MHz, CDCl3): δ = 10.0 (s, 1H, ArCHO), 7.90 (d, J = 8.0Hz, 2H, ArH), 7.63-7.67 (m, 1H, ArH), 7.53-7.57 (m, 2H, ArH); 13 CNMR (100MHz, CDCl3): δ = 192.5, 136.4, 134.5, 129.8, 129.0.
[0065] (2) Synthesis of compound 2b
[0066] 0.001 mol of 4-methoxystyrene 1b Dissolve in 2 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.003 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 8 hours, and wait until the reaction of raw material 1b is complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2b The yield was 93%. NMR spectrum data of compound 2b: 1 H NMR (400MHz, CDCl3): δ = 9.89 (s, 1H, ArCHO), 7.85 (d, J = 8.8Hz, 2H, ArH), 7.01 (d, J = 8.8Hz, 2H, ArH), 3.89 (s, 3H, ArCH3); 13 C NMR (100MHz, CDCl3): δ = 190.9, 164.6, 132.0, 129.9, 114.3, 55.6.
[0067] (3) Synthesis of compound 2c
[0068] 0.001 mol of 4-fluorostyrene 1c Dissolve in 2 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.003 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 8 hours, and wait for the reaction of raw material 1c to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2c The yield was 96%. NMR spectrum data of compound 2c: 1 H NMR (400MHz, CDCl3): δ = 9.98 (s, 1H, ArCHO), 7.90-7.94 (m, 2H, ArH), 7.22 (t, J = 8.4Hz, 2H, ArH); 13 C NMR (100MHz, CDCl3): δ=190.6, 167.8, 165.3, 132.9 (J=2.7Hz), 132.3 (J=9.8Hz), 116.5 (J=22.1Hz).
[0069] (4) Synthesis of compound 2d
[0070] 0.001 mol of 4-bromostyrene was added for 1 d Dissolve in 2 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.003 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 8 hours, and wait for the reaction of raw material 1d to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2d The yield was 92%. NMR spectrum data of compound 2d: 1 H NMR (400MHz, CDCl3): δ = 9.98 (s, 1H, ArCHO), 7.75-7.77 (m, 2H, ArH), 7.69-7.71 (m, 2H, ArH); 13 C NMR (100MHz, CDCl3): δ = 191.2, 135.1, 132.5, 131.0, 129.8.
[0071] (5) Synthesis of compound 2e
[0072] 0.001 mol of 1,1-diphenylethylene 1e Dissolved in 2 mL of ethanol, 0.1 mol% of zinc coordination polymer and 0.003 mol of hydrogen peroxide were added to the above solution, and the above mixture was moved to 60°C for 12 hours to react until the raw material 1e was completely reacted. Subsequently, ethyl acetate was added for extraction twice, 10 mL / time, and the solvent was drained. The crude product was separated by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate with a volume ratio of 20:1) to obtain compound 2e The yield was 97%. NMR spectrum data of compound 2e: 1 H NMR (400MHz, CDCl3): δ = 7.81 (d, J = 7.6Hz, 4H, ArH), 7.58-7.61 (m, 2H, ArH), 7.47-7.50 (m, 4H, ArH); 13 C NMR (100MHz, CDCl3): δ = 196.9, 137.6, 132.5, 130.1, 128.3.
[0073] The general structure of aryl-substituted ethylene is R of 1a~1e 1 and R 2 See Table 2.
[0074] Table 2
[0075]
[0076]
[0077] Example 2
[0078] A method for preparing a zinc coordination polymer:
[0079] Weigh 0.2mmol of isotribenzoic acid, 0.2mmol of 2,4,6-tris(4-pyridyl)-1,3,5-triazine and 0.4mmol of zinc nitrate hexahydrate, add them to a mixed solution containing 1mL of methanol and 3.5mL of N,N-dimethylacetamide, stir for 5 minutes under air atmosphere at room temperature, then transfer the stirred solution to a 15mL Teflon autoclave, heat to 110℃ in an oven and keep the temperature constant for 72 hours. After the reaction is completed, cool to room temperature at a rate of 15℃ / h to obtain pale yellow crystals, which are filtered, washed with methanol and vacuum dried for 2 hours to obtain zinc coordination polymer with a yield of 68%. Grind the obtained coordination polymer through a 100-mesh sieve and set aside.
[0080] The thermal stability of the zinc coordination polymer prepared in this example was characterized by a thermogravimetric analysis experiment. Specifically, the temperature was raised at a heating rate of 10°C / min under nitrogen purge to measure the thermal gravimetric curve of the zinc coordination polymer. The results are shown in Figure 6 It can be seen that the zinc coordination polymer product prepared in this example shows good thermal stability below 350° C., just like Example 1.
[0081] The zinc coordination polymer prepared in this example was subjected to XRD analysis, and the results are shown in Figure 7 It can be seen that the characteristic peaks of the XRD spectrum of powder diffraction are consistent with the characteristic peaks of theoretical simulation, indicating that the structure of the synthesized zinc coordination polymer is consistent with the simulated structure and is a pure phase.
[0082] Effect Example 2 (Taking the zinc coordination polymer prepared in Example 2 as an example)
[0083] Catalytic aryl substitution of ethylene to synthesize aryl formaldehyde / aryl ketone derivatives 2a~2f:
[0084] (1) Synthesis of compound 2a
[0085] 0.002 mol of styrene 1a Dissolve in 3 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.006 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 6 hours, and wait for the reaction of raw material 1a to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2a The yield was 93%. NMR spectrum data of compound 2a: 1 H NMR (400MHz, CDCl3): δ = 10.0 (s, 1H, ArCHO), 7.90 (d, J = 8.0Hz, 2H, ArH), 7.63-7.67 (m, 1H, ArH), 7.53-7.57 (m, 2H, ArH); 13 CNMR (100MHz, CDCl3): δ = 192.5, 136.4, 134.5, 129.8, 129.0.
[0086] (2) Synthesis of compound 2b
[0087] 0.002 mol of 4-methoxystyrene 1b Dissolve in 3 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.006 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 10 hours, and wait for the reaction of raw material 1b to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2b The yield was 94%. NMR spectrum data of compound 2b: 1 H NMR (400MHz, CDCl3): δ = 9.89 (s, 1H, ArCHO), 7.85 (d, J = 8.8Hz, 2H, ArH), 7.01 (d, J = 8.8Hz, 2H, ArH), 3.89 (s, 3H, ArCH3); 13 C NMR (100MHz, CDCl3): δ = 190.9, 164.6, 132.0, 129.9, 114.3, 55.6.
[0088] (3) Synthesis of compound 2c
[0089] 0.002 mol of 4-fluorostyrene 1c Dissolve in 3 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.006 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 10 hours, and wait for the reaction of raw material 1c to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate with a volume ratio of 20:1) to obtain compound 2c The yield was 97%. NMR spectrum data of compound 2c: 1H NMR (400MHz, CDCl3): δ = 9.98 (s, 1H, ArCHO), 7.90-7.94 (m, 2H, ArH), 7.22 (t, J = 8.4Hz, 2H, ArH); 13 C NMR (100MHz, CDCl3): δ=190.6, 167.8, 165.3, 132.9 (J=2.7Hz), 132.3 (J=9.8Hz), 116.5 (J=22.1Hz).
[0090] (4) Synthesis of compound 2d
[0091] 0.002 mol of 4-bromostyrene was added for 1 d Dissolve in 3 mL of ethanol, add 0.1 mol% zinc coordination polymer and 0.006 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 10 hours, and wait for the reaction of raw material 1d to be complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate in a volume ratio of 20:1) to obtain compound 2d The yield is 93%. NMR spectrum data of compound 2d: 1 H NMR (400MHz, CDCl3): δ = 9.98 (s, 1H, ArCHO), 7.75-7.77 (m, 2H, ArH), 7.69-7.71 (m, 2H, ArH); 13 C NMR (100MHz, CDCl3): δ = 191.2, 135.1, 132.5, 131.0, 129.8.
[0092] (5) Synthesis of compound 2e
[0093] 0.002 mol of 1,1-diphenylethylene 1e Dissolved in 3 mL of ethanol, 0.1 mol% of zinc coordination polymer and 0.006 mol of hydrogen peroxide were added to the above solution, and the above mixture was moved to 60°C for 10 hours to react until the raw material 1e was completely reacted. Subsequently, ethyl acetate was added for extraction twice, 10 mL / time, the solvent was drained, and the crude product was separated by column chromatography (first eluted with pure petroleum ether as eluent, and then eluted with petroleum ether and ethyl acetate with a volume ratio of 20:1) to obtain compound 2e The yield is 95%. NMR spectrum data of compound 2e: 1H NMR (400MHz, CDCl3): δ = 7.81 (d, J = 7.6Hz, 4H, ArH), 7.58-7.61 (m, 2H, ArH), 7.47-7.50 (m, 4H, ArH); 13 C NMR (100MHz, CDCl3): δ = 196.9, 137.6, 132.5, 130.1, 128.3.
[0094] Effect Example 3
[0095] The catalyst used in Example 2 to catalyze the synthesis of benzaldehyde 2a was subjected to three catalytic cycles under the same experimental conditions as above (the catalyst was collected by centrifugation after each reaction for the next reaction), and the yield of benzaldehyde 2a after each cycle was calculated. At the same time, the zinc coordination polymer after three catalytic cycles was characterized by X-ray powder diffraction. The results are shown in FIG. Figure 8 and Fig. 9 .from Figure 8 and Fig. 9 It can be seen that the catalytic activity of the zinc coordination polymer prepared in Example 2 has not changed substantially after three cycles of use, and the structure of the material also remains unchanged, indicating that the material has good chemical stability and catalytic stability.
[0096] Comparative Example 1
[0097] Directly use 2,4,6-tris(4-pyridyl)-1,3,5-triazine to catalyze the aryl substitution of ethylene to synthesize aryl formaldehyde / aryl ketone derivatives, wherein the structural formula of 2,4,6-tris(4-pyridyl)-1,3,5-triazine is as follows:
[0098]
[0099] The specific application method is:
[0100] 0.001 mol of styrene 1a Dissolve in 2 mL of ethanol, add 0.1 mol% 2,4,6-tris(4-pyridyl)-1,3,5-triazine and 0.003 mol of hydrogen peroxide to the above solution, move the above mixture to 60°C for 8 hours, and wait until the reaction of raw material 1a is complete. Then, add ethyl acetate to extract twice, 10 mL / time, drain the solvent, and separate the crude product by column chromatography (the specific process is the same as Example 1) to obtain compound 2a The yield is 38%. NMR spectrum data of compound 2a: 1H NMR (400MHz, CDCl3): δ = 10.0 (s, 1H, ArCHO), 7.90 (d, J = 8.0Hz, 2H, ArH), 7.63-7.67 (m, 1H, ArH), 7.53-7.57 (m, 2H, ArH); 13 C NMR (100MHz, CDCl3): δ = 192.5, 136.4, 134.5, 129.8, 129.0.
[0101] In this comparative example, 2,4,6-tris(4-pyridyl)-1,3,5-triazine is directly used as a catalyst. The yield of the reaction of catalyzing aromatic substituted ethylene to synthesize aromatic formaldehyde / aromatic ketone derivatives is significantly lower than that of the zinc coordination polymer prepared in Examples 1 to 2, indicating that the coordination of 2,4,6-tris(4-pyridyl)-1,3,5-triazine with zinc ions can significantly improve its catalytic activity.
[0102] Comparative Example 2
[0103] The same as step (1) of Example 1, except that the coordination polymer prepared in Example 2 is replaced by trimesic acid, that is, trimesic acid is directly used as a catalyst to catalyze the reaction of styrene 1a Conversion.
[0104] According to the results of H NMR and column chromatography, no benzaldehyde 2a was detected. This indicates that trimesic acid cannot catalyze the conversion of styrene into benzaldehyde.
[0105] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a zinc coordination polymer, characterized in that: The following steps are involved: Trimesic acid, 2,4,6-tris(4-pyridyl)-1,3,5-triazine and zinc nitrate hexahydrate are dissolved in a mixed solution of methanol and N,N-dimethylacetamide, and stirred evenly to obtain a solution. The solution is heated at 90-110° C. and cooled to room temperature to obtain light yellow crystals, which are the zinc coordination polymer.
2. The method for preparing a zinc coordination polymer according to claim 1, characterized in that: The molar ratio of trimesic acid, 2,4,6-tris(4-pyridyl)-1,3,5-triazine and zinc nitrate hexahydrate is 1:1:
2.
3. The method for preparing a zinc coordination polymer according to claim 1, characterized in that: The volume ratio of the methanol to N,N-dimethylacetamide is 1:(3-3.5).
4. The method for preparing a zinc coordination polymer according to claim 1, characterized in that: The heating time is 48 to 72 hours, and the cooling rate is 10 to 15° C. / min.
5. A zinc coordination polymer, characterized in that Obtained according to the preparation method according to any one of claims 1 to 4.
6. Use of the zinc coordination polymer according to claim 5 in catalyzing the conversion of aromatic substituted ethylene into aromatic formaldehyde / aromatic ketone derivatives.
7. The use according to claim 6, characterized in that: The aromatic substituted ethylene includes styrene and its derivatives.
8. A method for catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives, characterized in that: The aromatic substituted ethylene is dissolved in ethanol, and then the zinc coordination polymer and hydrogen peroxide described in claim 5 are added, and the obtained mixed solution is heated to 60° C. After the raw materials react completely, ethyl acetate is added for extraction, and the solvent is drained to obtain a crude product; the crude product is separated by column chromatography to obtain the aromatic formaldehyde / aromatic ketone derivative.
9. The method for catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives according to claim 8, characterized in that: The reaction time is 6 to 12 hours.
10. The method for catalyzing the conversion of aryl-substituted ethylene into aryl formaldehyde / aryl ketone derivatives according to claim 8, characterized in that: The molar ratio of the aromatic substituted ethylene to the hydrogen peroxide is 1:3.
Citation Information
Patent Citations
Method for manufacturing catalyst used for synthesizing benzaldehyde
CN101108367A
Catalytic method for preparing aldehyde / ketone through oxidation of alcohol-based compound by using molecular oxygen
CN108191619A
Lewis acid-base bifunctional catalyst and preparation method and application thereof
CN112473743A
Photochromic Cd complex based on 2-TPT and preparation method thereof
CN117777167A
Metal organic frameworks as catalysts and hydrocarbon oxidation methods thereof