Method for preparing hydrogel from waste cotton, hydrogel and application of hydrogel in drying treatment of landfill leachate

By combining hydrogel prepared by waste cotton with photothermal materials and combining photomolecular effects, the problems of high energy consumption and slow evaporation rate in waste drying and leachate treatment are solved, and fast and low-energy waste drying is achieved Effect.

CN119019751AActive Publication Date: 2024-11-26CHINA ROC FUTURE CO

Patent Information

Application Number
CN202411327327.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-26
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

The existing garbage drying and leachate treatment technologies consume a lot of energy, the evaporation rate is slow, making it difficult to quickly complete drying.

Method used

Use waste cotton to prepare hydrogels, and combine photothermal materials with hydrogels, use photons to crack water clusters and photomolecular effects to increase the evaporation rate, and form a hydrogel-vapor interface for light evaporation.

Benefits of technology

The rapid drying of garbage leachate is achieved, energy consumption is reduced, evaporation efficiency is improved, and processing speed is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005055768080000241
    Figure BDA0005055768080000241
  • Figure BDA0005055768080000251
    Figure BDA0005055768080000251
  • Figure BDA0005055768080000261
    Figure BDA0005055768080000261
Patent Text Reader

Abstract

The invention provides a method for preparing hydrogel from waste cotton, the hydrogel and application of the hydrogel in drying treatment of landfill leachate. The method comprises the following steps: carrying out bleaching treatment, alkalization reaction and etherification reaction on waste cotton to obtain sodium carboxymethyl cellulose; the preparation method comprises the following steps: carrying out hydrothermal reaction on graphene oxide, a sulfur source and a copper source to obtain a copper sulfide-reduced graphene oxide nano composite material; and carrying out a cross-linking reaction on sodium carboxymethyl cellulose, the copper sulfide-reduced graphene oxide nano composite material and a chitosan compound to obtain the dual-network hydrogel. The hydrogel can rapidly absorb and retain a large amount of water, the evaporation efficiency is remarkably improved, the hydrogel can be used for absorbing leachate on the surface of garbage, a hydrogel-steam interface can be rapidly formed, then illumination evaporation is conducted, and meanwhile the purposes of low energy consumption and high-speed drying of the garbage leachate are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of garbage drying, and in particular to a method for preparing hydrogel by using waste cotton, the hydrogel and application of the hydrogel in the drying treatment of garbage leachate. Background Art

[0002] In order to treat domestic waste, whether it is incineration or other thermal treatment processes such as pyrolysis and gasification, the original waste needs to be dried. During the drying process, the conventional treatment method is to use heating, which requires a lot of energy. The present application uses visible light to dry domestic waste. While using photothermal materials and hydrogels to evaporate water, photons can be combined to crack water from the hydrogel-steam interface and evaporate the water contained in the domestic waste. The synergistic effect completes the drying of the waste. The photothermal materials and hydrogels are combined and combined with the light molecular effect to evaporate the water in the domestic waste, so that the waste is dried and the energy consumption of waste drying is reduced.

[0003] When raw garbage is piled up and stored in garbage storage pools, a certain amount of leachate will be produced, which is difficult to separate completely. This requires drying the raw garbage based on the on-site environment of the garbage storage pool. The theory that the evaporation rate of water at the hydrogel-steam interface under specific visible light is higher than thermal evaporation is used, and an evaporator made of a composite of photothermal materials and hydrogels can be used to dry the garbage.

[0004] CN113149312A discloses a device and method for treating landfill leachate membrane separation concentrate by surface photothermal evaporation, belonging to the technical field of landfill leachate membrane concentrate treatment. It includes a condenser, a reaction tank, an evaporation table, a hydrophilic porous material layer, a photothermal porous material layer, an inclined transparent condensation top cover, a transparent side wall, a crystallized salt collection box, a condensed water collection tank and a condensed water outlet; the condenser is embedded in the inclined transparent condensation top cover; the inclined transparent condensation top cover and the transparent side wall cover are placed above the crystallized salt collection box; the reaction tank is placed in the crystallized salt collection box; the evaporation table is located at the edge of the reaction tank, and the evaporation table is attached to the hydrophilic porous material layer and the photothermal porous material layer from bottom to top in sequence, and the hydrophilic porous material layer extends to the side wall of the reaction tank. The reactor promotes air convection on the surface of the photothermal material through internal air circulation, and enhances the surface evaporation rate of the photothermal material. This method requires a layer of hydrophilic porous material to absorb water, and then a layer of photothermal material to catalyze the reaction to evaporate the water. In addition, the presence of a photocatalyst is required to promote the evaporation rate of the garbage surface, which means that it takes a relatively long time to complete the drying of the garbage.

[0005] CN215855213U discloses a garbage leachate treatment device, including a water reservoir, a photothermal evaporation ball and a light-transmitting cover, wherein the light-transmitting cover covers the outside of the water reservoir, the photothermal evaporation ball is laid in the water reservoir, a steam flow fan is correspondingly arranged on the upper side of the photothermal evaporation ball, a fresh water tank is arranged around the water reservoir, a condenser is also arranged in the light-transmitting cover, the condenser outlet pipe is connected to the water pump, and the condenser outlet pipe is connected to the water reservoir. The device uses a photothermal evaporation ball to utilize light energy and convert it into heat energy to heat and evaporate the leachate, and separates water, volatile small molecules and salt, heavy metals, suspended matter bacteria, etc. in the garbage leachate, but it only discloses that the photothermal evaporation ball is a spherical floating structure wrapped with a flexible nano black gold material, and the black gold material is mostly a graphene material loaded with metal. Although it can utilize light energy and convert it into heat energy to heat and evaporate the leachate, it does not have the adsorption capacity for liquid, which also leads to a slow leachate evaporation speed, and it takes a relatively long time to complete the drying of garbage.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing hydrogel using waste cotton, hydrogel and its application in the drying treatment of landfill leachate. The hydrogel prepared by the method of the present invention can effectively use photons to directly crack water clusters at the interface between the hydrogel and steam, and is composited with photothermal materials to prepare hydrogels. The evaporation rate is higher than that of commonly used hydrogel materials. It can be used to absorb leachate on the surface of garbage, quickly form a hydrogel-steam interface, and then perform light evaporation to achieve rapid drying of landfill leachate.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a method for preparing a hydrogel using waste cotton, the method comprising the following steps:

[0010] Waste cotton is bleached, alkalized and etherified to obtain sodium carboxymethyl cellulose;

[0011] The graphene oxide, the sulfur source and the copper source are subjected to a hydrothermal reaction to obtain a copper sulfide-reduced graphene oxide nanocomposite material;

[0012] Sodium carboxymethyl cellulose, copper sulfide-reduced graphene oxide nanocomposite and chitosan compounds are cross-linked to obtain a double network hydrogel.

[0013] In the present invention, sodium carboxymethyl cellulose is first prepared from waste cotton, and copper sulfide-reduced graphene oxide nanophotothermal materials are prepared at the same time, and then sodium carboxymethyl cellulose, copper sulfide-reduced graphene oxide nanophotothermal materials and chitosan compounds are cross-linked to obtain chitosan compounds-sodium carboxymethyl cellulose-CuS / rGO hydrogel, and finally impregnated in a solution containing an iron source to obtain a double network hydrogel. The hydrogel can absorb and retain a large amount of water, provide a humid environment for specific light-driven interfacial water evaporation, and improve evaporation efficiency. It can be used to absorb leachate on the surface of garbage, quickly form a hydrogel-vapor interface, and then perform light evaporation to achieve rapid drying of garbage leachate.

[0014] Among them, graphene oxide, sulfur source and copper source are hydrothermally reacted to obtain copper sulfide-reduced graphene oxide nanocomposite material; in the present application, the network of macroporous graphene oxide modified by copper sulfide has better porosity and high specific surface area, and the defective structure of CuS particles can lead to surface carrier migration, thereby forming a plasma resonance effect similar to that of precious metal nanoparticles to generate heat; in particular, the present application preferably uses acetylcysteine ​​as a sulfur source, and the acetyl group contained in it can better improve the binding ability of CuS and graphene oxide. And the copper sulfide-reduced graphene oxide nanocomposite material prepared by this method is more compatible with sodium carboxymethyl cellulose and chitosan compounds, so the present invention can be doped with photothermal material CuS-rGO in the hydrogel to improve the absorbance of the hydrogel, increase the photothermal effect of the hydrogel, and achieve rapid drying of landfill leachate.

[0015] Among them, after cross-linking of sodium carboxymethyl cellulose, copper sulfide-reduced graphene oxide nanocomposites and chitosan compounds, the resulting hydrogel has a large surface area and high porosity, which not only further improves the adsorption performance of the hydrogel, but also combines with the photomolecular effect to use light to efficiently evaporate the water at the hydrogel-air interface, and the evaporation efficiency is much higher than thermal evaporation.

[0016] Among them, the Fe 3+ As the central atom, sp 3 d 2 or 2 sp 3 Hybridization provides 6 empty orbitals, and the O in the carboxyl group can provide a lone pair of electrons, forming a coordination bond between the two, thereby achieving the bonding of sodium carboxymethyl cellulose and Fe 3+ coordination; when preparing hydrogel, metal ions coordinate with the carboxymethyl group in sodium carboxymethyl cellulose to cross-link it to form a three-dimensional spatial network structure, and wrap a large number of water molecules to form a hydrogel.

[0017] Preferably, the bleaching step comprises:

[0018] The waste cotton is soaked in an aqueous solution of hydrogen peroxide, and then washed, crushed and dried in sequence to obtain bleached waste cotton.

[0019] Preferably, the bleaching treatment temperature is 70-80°C, for example, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, etc., and the time is 20-40min, for example, 20min, 22min, 24min, 26min, 28min, 30min, 32min, 34min, 36min, 38min, 40min, etc.

[0020] Preferably, the content of hydrogen peroxide in the aqueous solution of hydrogen peroxide is 5-25wt%, for example, it can be 5wt%, 6wt%, 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 25wt% and the like.

[0021] Preferably, the bath ratio of the bleaching treatment is 1:(5-25), for example, it can be 1:5, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, 1:22, 1:24, 1:25, etc. (The bath ratio refers to the ratio of the mass of the waste cotton to the mass of the aqueous solution of hydrogen peroxide.)

[0022] Preferably, the alkalization step comprises:

[0023] The bleached waste cotton is placed in a sodium hydroxide solution for heating treatment and then dried to obtain alkali cellulose.

[0024] Preferably, the temperature of the alkalization reaction is 30-40°C, for example, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, etc., and the time is 1-3h, for example, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, etc.

[0025] Preferably, the content of sodium hydroxide in the sodium hydroxide solution is 30-40wt%, for example, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt% and the like.

[0026] Preferably, the solvent in the sodium hydroxide solution is a mixed solution of water and ethanol.

[0027] Preferably, the volume ratio of water to ethanol is (5-15):1, for example, it can be 5:1, 6:1, 8:1, 10:1, 12:1, 14:1, 15:1, etc.

[0028] Preferably, the bath ratio of the alkalization reaction is 1:(10-20), for example, 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, etc. (The bath ratio refers to the ratio of the mass of the bleached waste cotton to the mass of the sodium hydroxide solution.)

[0029] Preferably, the etherification reaction step comprises:

[0030] Alkali cellulose, chloroacetic acid and ethanol are mixed, reacted and then dried to obtain sodium carboxymethyl cellulose.

[0031] Preferably, the mass ratio of alkali cellulose, chloroacetic acid and ethanol is 1:(0.5-1.5):(5-15);

[0032] Here, “0.5-1.5” can be, for example, 0.5, 0.6, 0.8, 1, 1.2, 1.5, etc.;

[0033] Here, “5-15” can be, for example, 5, 6, 8, 10, 12, 14, 15, etc.

[0034] Preferably, the etherification reaction comprises: first reacting at 45-55°C (for example, 45°C, 46°C, 48°C, 50°C, 52°C, 54°C, 55°C, etc.) for 30-50min (for example, 30min, 32min, 34min, 36min, 38min, 40min, 42min, 44min, 46min, 48min, 50min, etc.), and then heating to 70-80°C (for example, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, etc.) for 1-2h (for example, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc.).

[0035] Preferably, the sodium carboxymethyl cellulose is prepared by the following steps:

[0036] S1. Bleaching treatment:

[0037] The waste cotton is placed in a 5-25wt% hydrogen peroxide aqueous solution, soaked at 70-80°C for 20-40 minutes, and then washed, crushed and dried in sequence to obtain bleached waste cotton.

[0038] S2. Alkalization reaction:

[0039] The bleached waste cotton is placed in a 30-40wt% sodium hydroxide ethanol aqueous solution, heated at 30-40°C for reaction for 1-3h, and then dried to obtain alkali cellulose.

[0040] S3, etherification reaction:

[0041] Alkali cellulose, chloroacetic acid and ethanol in a mass ratio of 1: (0.5-1.5): (5-15) are mixed, first reacted at 45-55°C for 30-50 minutes, then heated to 70-80°C for 1-2 hours, and then dried to obtain sodium carboxymethyl cellulose.

[0042] Preferably, the copper sulfide-reduced graphene oxide nanocomposite material is prepared by the following steps:

[0043] (a) dispersing graphene oxide in water, performing ultrasonic treatment to obtain a graphene oxide dispersion, and then adding a sulfur source and stirring to obtain a graphene oxide liquid containing a sulfur source;

[0044] (b) dissolving a copper source in water to obtain a copper source solution, and then adding the solution to the graphene oxide solution containing a sulfur source to obtain a raw material solution;

[0045] (c) placing the raw material liquid in a reaction kettle to carry out a hydrothermal reaction, and then washing and drying to obtain the copper sulfide-reduced graphene oxide nanocomposite material.

[0046] Preferably, the mass ratio of the graphene oxide, the sulfur source and the copper source is 1:(15-25):(1-10);

[0047] Here, “15-25” can be, for example, 15, 16, 18, 20, 22, 24, 25, etc.;

[0048] Here, “1-10” can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.

[0049] Preferably, the sulfur source is acetylcysteine.

[0050] Preferably, the copper source includes any one of copper chloride, copper sulfate, copper nitrate or copper acetate, or a combination of at least two thereof.

[0051] Preferably, in step (a), the power of the ultrasonic treatment is 100-200 W, for example, 100 W, 120 W, 140 W, 160 W, 180 W, 200 W, etc., and the time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, etc.

[0052] Preferably, in step (c), the temperature of the hydrothermal reaction is 100-200°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc., and the time is 5-15h, for example, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, etc.

[0053] Preferably, the graphene oxide is prepared by the following steps:

[0054] Graphite powder and concentrated sulfuric acid are mixed and stirred; potassium permanganate is added, stirred and reacted to obtain a reaction solution 1; water is added to the reaction solution 1 to dilute it, and then hydrogen peroxide is added to obtain a reaction solution 2; dilute hydrochloric acid is added to the reaction solution 2, and the reaction solution is allowed to stand overnight to obtain a crude product of graphene oxide; the crude product of graphene oxide is then washed and dried in sequence to obtain the graphene oxide (GO).

[0055] Preferably, the graphene oxide is prepared by the following steps:

[0056] Mix graphite powder and concentrated sulfuric acid, and stir for 30 to 50 minutes (for example, 30 minutes, 32 minutes, 34 minutes, 36 minutes, 38 minutes, 40 minutes, etc.) at a temperature below 5°C (for example, 5°C, 4°C, 3°C, 2°C, 1°C, 0°C, -1°C, -2°C, -3°C, -4°C, -5°C, -6°C, -8°C, -10°C, etc.);

[0057] After potassium permanganate is added, the mixture is stirred and reacted at 30-40° C. (for example, 30° C., 31° C., 32° C., 33° C., 34° C., 35° C., 36° C., 37° C., 38° C., 39° C., 40° C., etc.) for 2-4 hours to obtain a reaction solution 1;

[0058] Then, water is added to the reaction solution 1 to dilute it at a temperature below 5°C (for example, 5°C, 4°C, 3°C, 2°C, 1°C, 0°C, -1°C, -2°C, -3°C, -4°C, -5°C, -6°C, -8°C, -10°C, etc.), and then hydrogen peroxide is added until no bubbles emerge to obtain a reaction solution 2;

[0059] Then, dilute hydrochloric acid is added to the reaction solution 2 at a temperature below 35°C (for example, 35°C, 30°C, 25°C, 20°C, 15°C, 10°C, 5°C, etc.), and the reaction solution is allowed to stand for 6 to 18 hours (for example, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, etc.) at a temperature below 5°C (for example, 5°C, 4°C, 3°C, 2°C, 1°C, 0°C, -1°C, -2°C, -3°C, -4°C, -5°C, -6°C, -8°C, -10°C, etc.) to obtain a crude product of graphene oxide;

[0060] The crude graphene oxide product is then centrifugally washed with water until the pH value of the washing waste liquid is neutral, and the washed crude graphene oxide product is freeze-dried to obtain the graphene oxide (GO).

[0061] Preferably, the ratio of the mass of the graphite powder to the volume of concentrated sulfuric acid (98wt%) is 1g:(20-30)mL, for example, it can be 1g:20mL, 1g:22mL, 1g:24mL, 1g:25mL, 1g:26mL, 1g:28mL, 1g:30mL, etc.

[0062] Preferably, the mass ratio of the graphite powder to potassium permanganate is 1:(3-4), for example, it can be 1:3, 1:3.2, 1:3.4, 1:3.5, 1:3.6, 1:3.8, 1:4, etc.

[0063] Preferably, the ratio of the mass of the graphite powder to the volume of hydrogen peroxide (30wt%) is 1g:(8-12)mL, for example, it can be 1g:8mL, 1g:8.5mL, 1g:9mL, 1g:9.5mL, 1g:10mL, 1g:10.5mL, 1g:11mL, 1g:11.5mL, 1g:12mL, etc.

[0064] Preferably, the preparation method of the double network hydrogel comprises the following steps:

[0065] (A) mixing the sodium carboxymethyl cellulose and the copper sulfide-reduced graphene oxide nanocomposite with water respectively to obtain an aqueous solution of the sodium carboxymethyl cellulose and a dispersion of the copper sulfide-reduced graphene oxide nanocomposite; dissolving a chitosan compound in an acetic acid solution to obtain an acid solution of the chitosan compound;

[0066] (B) mixing the aqueous solution of sodium carboxymethyl cellulose, the dispersion of the copper sulfide-reduced graphene oxide nanocomposite material and the acid solution of the chitosan compound, and performing a cross-linking reaction under acidic conditions to obtain a cross-linked hydrogel.

[0067] Preferably, the mass ratio of the sodium carboxymethyl cellulose, the copper sulfide-reduced graphene oxide nanocomposite material and the chitosan compound is (5-8):(2-4):(1-3);

[0068] Here, “5-8” may be, for example, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc.;

[0069] Here, “2-4” can be, for example, 2, 2.5, 3, 3.5, 4, etc.;

[0070] Here, “1-3” can be, for example, 1, 1.5, 2, 2.5, 3, etc.

[0071] Preferably, the chitosan compound includes carboxymethyl chitosan.

[0072] Preferably, in step (B), hydrochloric acid needs to be added before the cross-linking reaction.

[0073] Preferably, in step (B), the concentration of the hydrochloric acid is 1.0 to 1.5 mol·L -1 , for example, it can be 1.0mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, etc.

[0074] Preferably, in step (B), the amount of hydrochloric acid added is 0.5-5% of the total mass of the mixed solution of the cross-linking reaction, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0075] Preferably, in step (B), a cross-linking agent needs to be added before the cross-linking reaction.

[0076] Preferably, in step (B), the cross-linking agent is glutaraldehyde.

[0077] Preferably, in step (B), the added amount of glutaraldehyde is 0.5-5% of the mass of the sodium carboxymethyl cellulose, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0078] Preferably, in step (B), the temperature of the cross-linking reaction is 20-40°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, etc., and the time is 6-18h, for example, 6h, 8h, 10h, 12h, 14h, 16h, 18h, etc.

[0079] Preferably, the method for preparing the double network hydrogel further comprises the following step, that is, the above step (B) further comprises the following step (C);

[0080] The cross-linked hydrogel is immersed in the solution containing the iron source, and then washed and dried to obtain a double network hydrogel.

[0081] Preferably, in step (C), the concentration of the solution containing the iron source is 0.1-1 mol / L, for example, it can be 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, etc.

[0082] Preferably, in step (C), the iron source comprises ferric chloride.

[0083] Preferably, in step (C), the immersion temperature is below 5°C, for example, 5°C, 4°C, 3°C, 2°C, 1°C, 0°C, etc., and the immersion time is 1 to 3 hours, for example, 1h, 1.5h, 2h, 2.5h, 3h, etc.

[0084] In a second aspect, the present invention provides a hydrogel, which is prepared by the method for preparing a hydrogel using waste cotton as described in the first aspect.

[0085] In a third aspect, the present invention provides a use of the hydrogel as described in the second aspect in the drying treatment of landfill leachate.

[0086] In the present invention, the hydrogel can be used in the drying treatment of landfill leachate. Not only can the photothermal material be combined with the hydrogel to increase the water evaporation rate, but also the theory of photomolecular effect can be used to cause the liquid to evaporate from the surface of the garbage without the need for heat. When light is irradiated to the interface where air and water meet, the water molecules can be decomposed and floated into the air, that is, evaporation can be caused without any heat source.

[0087] In a fourth aspect, the present invention provides a method for drying landfill leachate, the drying method comprising the following steps:

[0088] The hydrogel as described in the second aspect is dispersed in the landfill leachate and irradiated with light to evaporate the solution in the landfill leachate, thereby completing the drying of the landfill.

[0089] In the present invention, the double network hydrogel prepared by the above method can be dispersed in the landfill leachate and irradiated with visible light in a certain wavelength range. When the light evaporates the original garbage moisture, the air temperature tested above the leachate water surface is low and gradually tends to be stable, indicating that thermal energy is not the driving force behind it, and reaches a peak in green light, with the best drying effect. The photomolecular effect shows that photons can break up water clusters from the liquid surface and release them from the water-steam interface. When light is irradiated on the interface between air and water, it can knock water molecules away from the water surface and enter the air, thereby causing evaporation without any heat source. At the interface between water and air, light can directly evaporate water without heating, and it is more efficient than thermal evaporation. Based on this, an evaporator made of a composite of photothermal materials and hydrogels is used to further improve the evaporation efficiency.

[0090] When the leachate water molecules approach the surface of the double network hydrogel, they will be attracted by the hydrogel, thus forming a biased charge distribution, that is, the water molecules on the surface will have a positive charge, while the hydrogel will have a negative charge. In this way, a strong electric field gradient is formed on the surface of the hydrogel, which will produce a force on the water molecules, called a quadrupole force. The quadrupole force refers to when a dipole molecule is in a non-uniform electric field, it will be subjected to a force that makes its dipole moment consistent with the direction of the electric field. The magnitude and direction of this force depend on the gradient of the electric field and the shape of the dipole molecule. When photons are irradiated on the surface of the hydrogel, they are absorbed by the water molecules, thereby stimulating the vibration and rotation of the water molecules. These vibrations and rotations will change the dipole moment of the water molecules, thereby changing the quadrupole force they are subjected to. If the energy of the photons is large enough, they can make the quadrupole force of the water molecules exceed the attraction of the hydrogel, so that the water molecules are separated from the surface of the hydrogel. Because the hydrogen bonds between the water molecules are very strong, what is separated is not a single water molecule, but a water cluster, which can contain several to dozens of water molecules. These water clusters will fly away from the surface of the hydrogel, enter the air, and form water vapor, thereby reducing the moisture content of the original garbage.

[0091] Preferably, the wavelength of the light is 500-520 nm, for example, 500 nm, 510 nm, 515 nm, 520 nm, etc.

[0092] In the present invention, light with a certain range of wavelengths is used for irradiation. The results show that when the leachate level is higher than the original garbage, the evaporation rate is lower than the thermal limit, which belongs to the normal thermal evaporation stage. When the liquid level is lower than the sample surface, the evaporation rate exceeds the thermal evaporation limit. By testing light of different wavelengths, it is found that the evaporation rate in the range of 500-520nm is the highest.

[0093] Preferably, the intensity of the light is 0.5-2 kW / m 2 , for example, it can be 0.5kW / m 2 , 0.6kW / m 2 , 0.8kW / m 2 , 1kW / m 2 , 1.2kW / m 2 , 1.4kW / m 2 , 1.6kW / m 2 , 1.8kW / m 2 , 2kW / m 2 wait.

[0094] In a fifth aspect, the present invention provides a device for drying landfill leachate, wherein the device for drying landfill leachate comprises the hydrogel as described in the second aspect.

[0095] Preferably, the landfill leachate drying device comprises a landfill leachate evaporation tank; wherein the sidewalls and / or bottom of the landfill leachate evaporation tank are coated with a hydrogel layer formed by the hydrogel described in the second aspect.

[0096] Preferably, the landfill leachate drying device further comprises an evaporation table arranged at the edge of the landfill leachate evaporation pool; wherein the surface of the evaporation table is coated with a hydrogel layer formed by the hydrogel described in the second aspect.

[0097] Compared with the prior art, the present invention has the following beneficial effects:

[0098] (1) The present invention makes full use of the waste cotton in the original garbage to prepare the hydrogel, which has a large surface area and high porosity, good adsorption performance, and fully realizes the utilization of the waste cotton in the garbage.

[0099] (2) The present invention uses sodium carboxymethyl cellulose prepared from waste cotton, copper sulfide-reduced graphene oxide nanophotothermal material and chitosan compounds for cross-linking to obtain chitosan compound-sodium carboxymethyl cellulose-CuS / rGO hydrogel, and finally immerses it in a solution containing an iron source to obtain a double network hydrogel. The hydrogel can quickly absorb and retain a large amount of water, provide a humid environment for specific light-driven interfacial water evaporation, and significantly improve the evaporation efficiency. The hydrogel can be used to absorb the leachate on the surface of garbage, quickly form a hydrogel-vapor interface, and then perform light evaporation to achieve rapid drying of the garbage leachate.

[0100] (3) The present invention provides a method for treating landfill leachate, wherein a hydrogel material is dispersed in the original landfill leachate to form a hydrogel-steam interface layer, and a visible light emitting diode is arranged above the landfill storage tank to irradiate the hydrogel-steam interface layer in the landfill storage tank, so that the evaporation efficiency is higher than the thermal evaporation efficiency. DETAILED DESCRIPTION

[0101] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0102] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0103] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0104] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0105] Preparation Example 1

[0106] This preparation example provides a graphene oxide, which is prepared by the following steps:

[0107] Take 2g of graphite powder and 50mL of concentrated sulfuric acid (98%) and add them to a 500mL three-necked flask, stir in an ice bath for 40min, then add 7g of potassium permanganate to the three-necked flask in batches, after adding, transfer the flask to a 35°C oil bath and stir for 3h, at which time the reaction system is a dark green viscous liquid; then transfer the three-necked flask to an ice bath, add 180mL of deionized water to the three-necked flask under ice bath conditions, the reaction system is brown-yellow, and then add 20mL of hydrogen peroxide (3 0%) until no bubbles emerge, and the reaction system appears bright yellow; then the mixed solution in the three-necked flask is transferred to a 1000mL beaker, 100mL of dilute hydrochloric acid (10wt%) is added, and the mixture is allowed to stand overnight to obtain a crude product of graphene oxide; the crude product of graphene oxide is then centrifuged and washed with water until the pH value of the washing waste liquid is neutral to obtain a viscous dark brown product, and finally the viscous dark brown product is freeze-dried with a freeze dryer to obtain the product graphene oxide (GO).

[0108] Example 1

[0109] This embodiment provides a method for preparing a hydrogel using waste cotton, the method comprising the following steps:

[0110] S1. Bleaching treatment:

[0111] The waste cotton was placed in a 15wt% hydrogen peroxide aqueous solution with a bath ratio of 1:15, soaked at 75°C for 30 minutes, rinsed with distilled water for 3 times to remove impurities, crushed and dried to obtain bleached waste cotton.

[0112] S2. Alkalization reaction:

[0113] The bleached waste cotton was placed in a 35wt% sodium hydroxide ethanol aqueous solution (V 水 :V 乙醇=9:1), the bath ratio is 1:15, the reaction is heated at 35°C for 2h, and then dried to obtain alkali cellulose.

[0114] S3, etherification reaction:

[0115] Alkali cellulose, chloroacetic acid and ethanol in a mass ratio of 1:1.2:10 were mixed, first reacted at 50°C for 40 minutes, then heated to 75°C and reacted for 1.5 hours to obtain sodium carboxymethyl cellulose, which was then dried to obtain sodium carboxymethyl cellulose powder.

[0116] S4. Preparation of hydrogel:

[0117] S4-1. Preparation of copper sulfide-reduced graphene oxide nanocomposite (CuS-rGO):

[0118] (a) dispersing 0.2 g of the graphene oxide provided in Preparation Example 1 in 200 mL of deionized water, ultrasonicating at a power of 150 W for 2 h to obtain a 1 mg / mL graphene oxide dispersion, then adding 4 g of acetylcysteine ​​to the graphene oxide dispersion and stirring until it is completely dissolved to obtain a graphene oxide solution containing acetylcysteine;

[0119] (b) dissolving 1 g of copper chloride in 9 mL of deionized water, and slowly adding the graphene oxide solution containing acetylcysteine ​​to obtain a raw material solution;

[0120] (c) The raw material solution is placed in a reactor and reacted at 150°C for 10 h. The product is then washed three times with anhydrous ethanol and deionized water respectively. The washed product is freeze-dried to obtain CuS-rGO.

[0121] S4-2. Preparation of double network hydrogel:

[0122] (A) Weigh 6 g of sodium carboxymethyl cellulose and mix with 600 mL of deionized water to obtain an aqueous solution of sodium carboxymethyl cellulose; weigh 3 g of CuS-rGO and disperse it in 300 mL of deionized water to obtain a dispersion of CuS-rGO; weigh 1 g of carboxymethyl chitosan and mix with 100 mL of 0.2 mol / L acetic acid aqueous solution to obtain an acid solution of carboxymethyl chitosan;

[0123] (B) mixing the aqueous solution of sodium carboxymethyl cellulose, the dispersion of the copper sulfide-reduced graphene oxide nanocomposite and the acid solution of carboxymethyl chitosan, adding 2wt% 1.2mol / L aqueous hydrochloric acid solution and stirring for 3h, then adding 0.12g of glutaraldehyde, and standing at room temperature for crosslinking for 12h to obtain a crosslinked hydrogel;

[0124] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0125] Example 2

[0126] This embodiment provides a method for preparing a hydrogel using waste cotton, the method comprising the following steps:

[0127] S1. Bleaching treatment:

[0128] The waste cotton was placed in a 10wt% hydrogen peroxide aqueous solution with a bath ratio of 1:20, soaked at 70°C for 40 minutes, rinsed with distilled water for 3 times to remove impurities, crushed and dried to obtain bleached waste cotton.

[0129] S2. Alkalization reaction:

[0130] The bleached waste cotton was placed in a 30wt% sodium hydroxide ethanol aqueous solution (V 水 :V 乙醇 =9:1), the bath ratio is 1:20, the reaction is heated at 30°C for 3h, and dried to obtain alkali cellulose.

[0131] S3, etherification reaction:

[0132] Alkali cellulose, chloroacetic acid and ethanol in a mass ratio of 1:1.5:15 were mixed, first reacted at 45°C for 45 minutes, then heated to 70°C and reacted for 2 hours to obtain sodium carboxymethyl cellulose, which was then dried to obtain sodium carboxymethyl cellulose powder.

[0133] S4. Preparation of hydrogel:

[0134] S4-1. Preparation of copper sulfide-reduced graphene oxide nanocomposite (CuS-rGO):

[0135] (a) dispersing 0.2 g of the graphene oxide provided in Preparation Example 1 in 200 mL of deionized water, ultrasonicating at a power of 150 W for 2 h to obtain a 1 mg / mL graphene oxide dispersion, then adding 4 g of acetylcysteine ​​to the graphene oxide dispersion and stirring until it is completely dissolved to obtain a graphene oxide solution containing acetylcysteine;

[0136] (b) dissolving 1 g of copper chloride in 9 mL of deionized water, and slowly adding the graphene oxide solution containing acetylcysteine ​​to obtain a raw material solution;

[0137] (c) The raw material solution is placed in a reactor and reacted at 120°C for 12 h. The product is then washed three times with anhydrous ethanol and deionized water respectively. The washed product is freeze-dried to obtain CuS-rGO.

[0138] S4-2. Preparation of double network hydrogel:

[0139] (A) Weigh 5 g of sodium carboxymethyl cellulose and mix with 500 mL of deionized water to obtain an aqueous solution of sodium carboxymethyl cellulose; weigh 2 g of CuS-rGO and disperse it in 200 mL of deionized water to obtain a dispersion of CuS-rGO; weigh 3 g of carboxymethyl chitosan and mix with 300 mL of 0.2 mol / L acetic acid aqueous solution to obtain an acid solution of carboxymethyl chitosan;

[0140] (B) mixing the aqueous solution of sodium carboxymethyl cellulose, the dispersion of the copper sulfide-reduced graphene oxide nanocomposite and the acid solution of carboxymethyl chitosan, adding 2wt% 1.2mol / L aqueous hydrochloric acid solution and stirring for 3h, then adding 0.1g glutaraldehyde, and standing at room temperature for crosslinking for 12h to obtain a crosslinked hydrogel;

[0141] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0142] Example 3

[0143] This embodiment provides a method for preparing a hydrogel using waste cotton, the method comprising the following steps:

[0144] S1. Bleaching treatment:

[0145] The waste cotton was placed in a 20wt% hydrogen peroxide aqueous solution with a bath ratio of 1:25, soaked at 80°C for 20 minutes, rinsed with distilled water for 3 times to remove impurities, crushed and dried to obtain bleached waste cotton.

[0146] S2. Alkalization reaction:

[0147] The bleached waste cotton was placed in a 40wt% sodium hydroxide ethanol aqueous solution (V 水 :V 乙醇 =9:1), the bath ratio is 1:10, the reaction is heated at 40°C for 1 hour, and then dried to obtain alkali cellulose.

[0148] S3, etherification reaction:

[0149] Alkali cellulose, chloroacetic acid and ethanol in a mass ratio of 1:0.8:8 were mixed, first reacted at 55°C for 30 minutes, then heated to 80°C and reacted for 1 hour to obtain sodium carboxymethyl cellulose, which was then dried to obtain sodium carboxymethyl cellulose powder.

[0150] S4. Preparation of hydrogel:

[0151] S4-1. Preparation of copper sulfide-reduced graphene oxide nanocomposite (CuS-rGO):

[0152] (a) dispersing 0.2 g of the graphene oxide provided in Preparation Example 1 in 200 mL of deionized water, ultrasonicating at a power of 150 W for 2 h to obtain a 1 mg / mL graphene oxide dispersion, then adding 4 g of acetylcysteine ​​to the graphene oxide dispersion and stirring until it is completely dissolved to obtain a graphene oxide solution containing acetylcysteine;

[0153] (b) dissolving 1 g of copper chloride in 9 mL of deionized water, and slowly adding the graphene oxide solution containing acetylcysteine ​​to obtain a raw material solution;

[0154] (c) The raw material solution is placed in a reactor and reacted at a constant temperature of 180°C for 8 hours. The product is then washed three times with anhydrous ethanol and deionized water respectively. The washed product is freeze-dried to obtain CuS-rGO.

[0155] S4-2. Preparation of double network hydrogel:

[0156] (A) 7 g of sodium carboxymethyl cellulose was mixed with 700 mL of deionized water to obtain an aqueous solution of sodium carboxymethyl cellulose; 2 g of CuS-rGO was dispersed in 200 mL of deionized water to obtain a dispersion of CuS-rGO; 1 g of carboxymethyl chitosan was mixed with 100 mL of 0.2 mol / L acetic acid aqueous solution to obtain an acid solution of carboxymethyl chitosan;

[0157] (B) mixing the aqueous solution of sodium carboxymethyl cellulose, the dispersion of the copper sulfide-reduced graphene oxide nanocomposite and the acid solution of carboxymethyl chitosan, adding 2wt% 1.2mol / L aqueous hydrochloric acid solution and stirring for 3h, then adding 0.14g glutaraldehyde, and standing at room temperature for crosslinking for 12h to obtain a crosslinked hydrogel;

[0158] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0159] Example 4

[0160] This embodiment provides a method for preparing a hydrogel using waste cotton, which is different from Example 1 only in that 4 g of acetylcysteine ​​in step (a) of S4-1 is replaced by 4 g of L-cysteine, and the other steps are exactly the same as Example 1.

[0161] Example 5

[0162] This embodiment provides a method for preparing a hydrogel using waste cotton, which is different from Embodiment 1 only in that the preparation method of S4-1, copper sulfide-reduced graphene oxide nanocomposite material (CuS-rGO) is different, as shown below:

[0163] Weigh 20 mg of graphene oxide and place it in 30 mL of ethanol. Ultrasonicate at a power of 150 W for 2 hours to obtain a graphene oxide dispersion, and then add 15 mmol urea, 0.1 mmol copper chloride and 0.1 mmol thiourea respectively; then place the above raw material liquid in a reactor and react at 160°C for 12 hours; then wash the product with anhydrous ethanol and deionized water for 3 times respectively, and the washed product will be freeze-dried to obtain CuS-rGO.

[0164] Example 6

[0165] This embodiment provides a method for preparing a hydrogel using waste cotton. The only difference from Example 1 is that 1 g of carboxymethyl chitosan in step (A) of S4-2 is replaced by 1 g of hydroxypropyl chitosan, and the other steps are exactly the same as Example 1.

[0166] Example 7

[0167] This embodiment provides a method for preparing a hydrogel using waste cotton, which is different from Example 1 only in that 1 g of carboxymethyl chitosan in step (A) of S4-2 is replaced by 1 g of chitosan, and the other steps are exactly the same as Example 1.

[0168] Example 8

[0169] This embodiment provides a method for preparing a hydrogel using waste cotton, which differs from Example 1 only in that the 0.5 mol / L aqueous solution of ferric chloride in step (C) of S4-2 is replaced by a 0.5 mol / L aqueous solution of cupric chloride, and the other steps are exactly the same as Example 1.

[0170] Example 9

[0171] This embodiment provides a method for preparing a hydrogel using waste cotton, which is different from Example 1 only in that the operation of impregnating the aqueous solution of ferric chloride in step (C) of S4-2 is no longer performed, but the cross-linked hydrogel is directly placed in a -20°C refrigerator for 12 hours and then placed in a freeze dryer for freeze drying for 48 hours to completely remove the moisture in the hydrogel. The other steps are exactly the same as in Example 1.

[0172] Comparative Example 1

[0173] This comparative example provides a method for preparing a hydrogel using waste cotton, the method comprising the following steps:

[0174] S1~S3: completely consistent with Example 1.

[0175] S4. Preparation of hydrogel:

[0176] (A) 6 g of sodium carboxymethyl cellulose was weighed and mixed with 600 mL of deionized water to obtain an aqueous solution of sodium carboxymethyl cellulose; 1 g of carboxymethyl chitosan was weighed and mixed with 100 mL of 0.2 mol / L acetic acid aqueous solution to obtain an acid solution of carboxymethyl chitosan;

[0177] (B) mixing the aqueous solution of sodium carboxymethyl cellulose and the acid solution of carboxymethyl chitosan, adding 2wt% 1.2mol / L aqueous hydrochloric acid solution and stirring for 3h, then adding 0.1g glutaraldehyde, and standing at room temperature for cross-linking for 12h to obtain a cross-linked hydrogel;

[0178] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0179] Comparative Example 2

[0180] This comparative example provides a method for preparing a hydrogel, the method comprising the following steps:

[0181] S1. Weigh 3 g of CuS-rGO and disperse it in 300 mL of deionized water to obtain a CuS-rGO dispersion; weigh 7 g of carboxymethyl chitosan and mix it with 100 mL of 0.2 mol / L acetic acid aqueous solution to obtain an acid solution of carboxymethyl chitosan;

[0182] S2, after mixing the dispersion of the copper sulfide-reduced graphene oxide nanocomposite material and the acid solution of carboxymethyl chitosan, add 2wt% 1.2mol / L hydrochloric acid aqueous solution and stir for 3h, then add 0.05g glutaraldehyde, stand for crosslinking at room temperature for 12h, to obtain a crosslinked hydrogel;

[0183] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0184] Comparative Example 3

[0185] This comparative example provides a method for preparing a hydrogel, the method comprising the following steps:

[0186] S1~S3: completely consistent with Example 1.

[0187] S4. Preparation of hydrogel:

[0188] S4-1. Preparation of copper sulfide-reduced graphene oxide nanocomposite material (CuS-rGO): completely consistent with Example 1.

[0189] S4-2. Preparation of double network hydrogel:

[0190] (A) 7 g of sodium carboxymethyl cellulose was weighed and mixed with 600 mL of deionized water to obtain an aqueous solution of sodium carboxymethyl cellulose; 3 g of CuS-rGO was weighed and dispersed in 300 mL of deionized water to obtain a CuS-rGO dispersion;

[0191] (B) mixing the aqueous solution of sodium carboxymethyl cellulose and the dispersion of copper sulfide-reduced graphene oxide nanocomposite, adding 2wt% 1.2mol / L aqueous hydrochloric acid solution and stirring for 3h, then adding 0.14g glutaraldehyde, and standing at room temperature for crosslinking for 12h to obtain a crosslinked hydrogel;

[0192] (C) The cross-linked hydrogel is placed in a 0.5 mol / L aqueous solution of ferric chloride and immersed at 0°C for 2 hours. The loaded cross-linked hydrogel is then taken out and the gel is subsequently rinsed with deionized water for 3 times to remove unreacted substances and excess salt solution. The gel is first frozen in a -20°C refrigerator for 12 hours and then freeze-dried in a freeze dryer for 48 hours to completely remove the moisture in the hydrogel to obtain the double network hydrogel.

[0193] Comparative Example 4

[0194] This comparative example provides a method for preparing a hydrogel, which differs from Example 1 in that 6 g of sodium carboxymethyl cellulose in step (A) of S4-2 is replaced by 6 g of sodium alginate of the same mass, and the other steps are exactly the same as those in Example 1.

[0195] Comparative Example 5

[0196] This comparative example provides a method for preparing a hydrogel, which differs from Example 1 in that 3 g of CuS-rGO in step (A) of S4-2 is replaced by 3 g of TiO 2 -rGO, the TiO 2 -rGO was prepared by the following steps:

[0197] (i) 0.2 g of the graphene oxide provided in Preparation Example 1 was dispersed in 200 mL of deionized water, and ultrasonicated at a power of 150 W for 2 h to obtain a 1 mg / mL graphene oxide dispersion; 0.5 g of titanium dioxide powder was weighed and dispersed in 50 mL of anhydrous ethanol, and ultrasonicated at a power of 150 W for 30 min to obtain a titanium dioxide dispersion;

[0198] (ii) mixing the graphene oxide dispersion and the titanium dioxide dispersion, and then slowly adding ammonia water until the pH value of the solution in the mixer reaches 10, thereby obtaining a raw material solution;

[0199] (iii) placing the raw material solution in a reaction kettle and maintaining it at 200° C. for 12 h. After the reaction is completed, cooling it to room temperature, and then washing the product with anhydrous ethanol and deionized water for three times respectively. The washed product is freeze-dried to obtain the TiO 2 -rGO;

[0200] The other steps are exactly the same as those in Example 1.

[0201] Comparative Example 6

[0202] This comparative example provides a method for preparing a hydrogel, which differs from Example 1 in that 1 g of carboxymethyl chitosan in step (A) of S4-2 is replaced with 1 g of polyvinyl alcohol of the same mass, and the other steps are completely consistent with Example 1.

[0203] Test Example 1

[0204] Test samples: hydrogels prepared in Examples 1 to 9 and hydrogels prepared in Comparative Examples 1 to 6.

[0205] Test method: Under the irradiation of sunlight of one intensity, the surface temperature change, water absorption swelling degree and solar heating water evaporation rate of each of the above hydrogels were tested; wherein, water absorption swelling degree (%) = [(mass of gel after water absorption - initial mass of gel) / initial mass of gel] × 100%.

[0206] The specific test results are shown in Table 1 below:

[0207] Table 1

[0208]

[0209]

[0210] As shown in Table 1, the surface temperature of the hydrogels prepared in Examples 1 to 9 increased by 20.1 to 39.7°C under the irradiation of one sunlight intensity, and the hydrogels had good photothermal conversion efficiency. The water absorption swelling degree of the hydrogels of the present invention was 12.23 to 19.51%, and the photothermal evaporation rate was 2.423 to 3.531 kg·m -1 ·h -1 This shows that the hydrogel of the present invention has excellent light-to-heat conversion efficiency and excellent water absorption performance.

[0211] Test Example 2

[0212] Test samples: hydrogels prepared in Examples 1 to 9 and hydrogels prepared in Comparative Examples 1 to 6.

[0213] Test method: The hydrogels were dispersed in evaporation ponds containing landfill leachate and irradiated with light (wavelength 510 nm, intensity 0.5 kW / m 2 ) to evaporate the solution in the leachate and complete the drying of the garbage.

[0214] The specific test results are shown in Table 2 below:

[0215] Table 2

[0216]

[0217]

[0218] As shown in Table 2, the energy required to convert the liquid water in the hydrogel leachate prepared in Examples 1 to 9 into gaseous water at the same temperature is only 0.318×10 6 ~0.336×10 6 J, evaporation rate is 17.2~23.6L·m -1 ·h -1 The daily amount of landfill leachate treated per unit area is 137.6 to 188.8 L·m -2 ·d -1, the photothermal conversion efficiency is 92.1-97.7%. This shows that the hydrogel of the present invention can quickly absorb and retain a large amount of water, provide a humid environment for the interfacial water evaporation driven by specific light, and significantly improve the evaporation efficiency. It can be used to absorb the leachate on the surface of garbage, quickly form a hydrogel-steam interface, and then perform light evaporation, while achieving the purpose of low energy consumption and high-speed drying of garbage leachate.

[0219] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing hydrogel using waste cotton, characterized in that: The method comprises the following steps: Waste cotton is bleached, alkalized and etherified to obtain sodium carboxymethyl cellulose; The graphene oxide, the sulfur source and the copper source are subjected to a hydrothermal reaction to obtain a copper sulfide-reduced graphene oxide nanocomposite material; Sodium carboxymethyl cellulose, copper sulfide-reduced graphene oxide nanocomposite and chitosan compounds are cross-linked to obtain a double network hydrogel.

2. The method for preparing hydrogel using waste cotton according to claim 1, characterized in that: The bleaching process comprises: The waste cotton is soaked in an aqueous solution of hydrogen peroxide, and then washed, crushed and dried in sequence to obtain bleached waste cotton; Preferably, the bleaching treatment is carried out at a temperature of 70 to 80°C and for a time of 20 to 40 minutes; Preferably, the content of hydrogen peroxide in the aqueous solution of hydrogen peroxide is 5 to 25 wt%; Preferably, the bath ratio of the bleaching treatment is 1:(5-25).

3. The method for preparing hydrogel using waste cotton according to claim 1, characterized in that: The steps of the alkalization reaction include: The bleached waste cotton is placed in a sodium hydroxide solution for heating treatment, and then dried to obtain alkali cellulose; Preferably, the alkalization reaction temperature is 30-40°C and the time is 1-3h; Preferably, the content of sodium hydroxide in the sodium hydroxide solution is 30-40wt%; Preferably, the solvent in the sodium hydroxide solution is a mixed solution of water and ethanol; Preferably, the volume ratio of water to ethanol is (5-15):1; Preferably, the bath ratio of the alkalization reaction is 1:(10-20).

4. The method for preparing hydrogel using waste cotton according to claim 1, characterized in that: The steps of the etherification reaction include: Alkali cellulose, chloroacetic acid and ethanol are mixed, reacted and then dried to obtain sodium carboxymethyl cellulose; Preferably, the mass ratio of alkali cellulose, chloroacetic acid and ethanol is 1:(0.5-1.5):(5-15); Preferably, the etherification reaction comprises: first reacting at 45-55° C. for 30-50 minutes, and then heating to 70-80° C. for 1-2 hours.

5. The method for preparing hydrogel using waste cotton according to claim 1, characterized in that: The copper sulfide-reduced graphene oxide nanocomposite material is prepared by the following steps: Dispersing graphene oxide in water, performing ultrasonic treatment to obtain a graphene oxide dispersion, and then adding a sulfur source and stirring to obtain a graphene oxide liquid containing a sulfur source; Dissolving a copper source in water to obtain a copper source solution, and then adding the solution to the graphene oxide solution containing a sulfur source to obtain a raw material solution; Placing the raw material liquid in a reaction kettle for hydrothermal reaction, and then washing and drying to obtain the copper sulfide-reduced graphene oxide nanocomposite material; Preferably, the mass ratio of the graphene oxide, the sulfur source and the copper source is 1:(15-25):(1-10); Preferably, the sulfur source is acetylcysteine; Preferably, the copper source includes any one or a combination of at least two of copper chloride, copper sulfate, copper nitrate or copper acetate; Preferably, the power of the ultrasonic treatment is 100-200W, and the time is 1-3h; Preferably, the temperature of the hydrothermal reaction is 100-200° C., and the time is 5-15 hours.

6. The method for preparing hydrogel using waste cotton according to claim 1, characterized in that: The preparation method of the double network hydrogel comprises the following steps: The sodium carboxymethyl cellulose and the copper sulfide-reduced graphene oxide nanocomposite are mixed with water respectively to obtain an aqueous solution of the sodium carboxymethyl cellulose and a dispersion of the copper sulfide-reduced graphene oxide nanocomposite; a chitosan compound is dissolved in an acetic acid solution to obtain an acid solution of the chitosan compound; The aqueous solution of sodium carboxymethyl cellulose, the dispersion of the copper sulfide-reduced graphene oxide nanocomposite material and the acid solution of the chitosan compound are mixed, and then cross-linked under acidic conditions to obtain a cross-linked hydrogel; Preferably, the mass ratio of the sodium carboxymethyl cellulose, the copper sulfide-reduced graphene oxide nanocomposite material and the chitosan compound is (5-8):(2-4):(1-3); Preferably, the chitosan compound comprises carboxymethyl chitosan; Preferably, hydrochloric acid needs to be added before the cross-linking reaction; Preferably, a cross-linking agent needs to be added before the cross-linking reaction; Preferably, the cross-linking agent is glutaraldehyde; Preferably, the added amount of glutaraldehyde is 0.5-5% of the mass of the sodium carboxymethyl cellulose; Preferably, the cross-linking reaction temperature is 20 to 40°C and the time is 6 to 18 hours; Preferably, the method for preparing the double network hydrogel further comprises the following steps: The cross-linked hydrogel is immersed in a solution containing an iron source, and then washed and dried to obtain a double network hydrogel; Preferably, the concentration of the solution containing the iron source is 0.1 to 1 mol / L; Preferably, the iron source comprises ferric chloride; Preferably, the immersion temperature is below 5°C and the time is 1 to 3 hours.

7. A hydrogel, characterized in that: The hydrogel is prepared by the method for preparing hydrogel using waste cotton as described in any one of claims 1 to 6.

8. Use of the hydrogel according to claim 7 in the drying treatment of landfill leachate.

9. A method for drying landfill leachate, characterized in that: The drying method comprises the following steps: Dispersing the hydrogel as claimed in claim 7 in landfill leachate, and irradiating the landfill leachate with light to evaporate the solution in the landfill leachate, thereby completing the drying of the landfill; the light irradiation is natural light or light at a specific wavelength; Preferably, the wavelength of the light is 500-520 nm; Preferably, the intensity of the light is 0.5-2 kW / m 2 .

10. A device for drying landfill leachate, characterized in that: The landfill leachate drying device comprises the hydrogel according to claim 7; Preferably, the landfill leachate drying device comprises a landfill leachate evaporation tank; wherein the sidewall and / or bottom of the landfill leachate evaporation tank is coated with a hydrogel layer formed by the hydrogel according to claim 7; Preferably, the landfill leachate drying device further comprises an evaporation table arranged at the edge of the landfill leachate evaporation pool; wherein the surface of the evaporation table is coated with a hydrogel layer formed by the hydrogel according to claim 7.

Citation Information

Patent Citations

  • Preparation method of instant sodium carboxymethyl cellulose

    CN112679620A

  • Nanocellulose-based solar interface evaporation device and preparation method and application thereof

    CN118598251A

  • A polymer nanocomposite membrane and a method of preparation thereof

    IN201821045962A

Cited By

  • Using a light device, in a drying device, for drying and / or at least enhancing of drying a product, drying assembly for drying a product, method for drying a product, drying part for a paper machine and paper machine comprising a drying part

    EP4814423A1