Sponge product and preparation method thereof
By forming an interpenetrating network structure through a low-temperature reaction between natural plant fibers and acrylic monomers, the problems of insufficient safety and softness in synthetic fiber sponge products are solved, and sponge products with high durability and cleaning ability are prepared, achieving a simple and efficient preparation process.
Patent Information
- Application Number
- CN202411496012.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-25
AI Technical Summary
Existing synthetic fiber sponge products have superior durability and cleaning ability, but poor safety and softness. Natural fiber sponge products, on the other hand, have good safety and softness, but limited cleaning ability. Modified natural fiber sponge products also have many shortcomings.
Using natural plant fibers as raw materials, the sponge is formed by reacting with acrylic monomers after swelling treatment with hydrogen peroxide. The low-temperature polymerization process is controlled to form an interpenetrating network structure. Combined with ultrasonic immersion technology, sponge products with high structural stability and good cleaning ability are prepared.
It achieves high affinity and softness of natural fiber sponges, while enhancing durability and cleaning power. The preparation process is simple, efficient, environmentally friendly and safe.
Smart Images

Figure CN119019753A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sponge products, and in particular to a sponge product and a preparation method thereof. Background Art
[0002] Sponge is a very common and commonly used product for cleaning. It is mostly used for cleaning kitchen utensils or cleaning the human body. These two uses have significantly different requirements for sponges. For example, kitchen utensil cleaning usually requires higher durability of the sponge, requiring higher hardness and sponge density to improve the cleaning effect, while for human body cleaning, there are higher requirements in affinity and softness.
[0003] Therefore, at present, most sponge products for cleaning are divided into synthetic sponges and natural sponges. Synthetic sponges have the characteristics of low cost, high cost performance, generally stronger durability and relatively higher hardness, and are used for cleaning kitchen utensils, while natural sponges have higher affinity to the human body, are softer, and are not easy to cause damage to the human epidermis or cause allergies, and are often used for human cleaning. However, with the development of natural sponges and people's increasing demand for the safety of cleaning sponges, more and more natural sponges are now used for cleaning kitchen utensils.
[0004] However, most of the existing natural sponges for cleaning kitchen utensils are wood pulp sponges or bamboo fiber sponges. In order to solve the defects of wood pulp sponges being easy to mildew and bamboo fiber sponges being poor in wear resistance and having a short service life, as well as the problem that wood pulp fiber and bamboo fiber are difficult to effectively construct a sponge body with a rich pore structure by themselves, most of them use a large amount of additives and regulators to construct a sponge body through auxiliary foaming with additives, regulators, etc., and use a large amount of adhesives. The actual safety and softness are relatively limited, and the water retention is relatively poor, and it is easy to lose water and dry. The adsorption and dispersion capacity of water and detergents is insufficient, and the actual cleaning effect is relatively limited. Therefore, for natural fiber sponges, it is still urgent to optimize and improve their performance. As for the current process, some processes are to modify plant fibers to make them have the durability of synthetic fibers, but they only enhance durability, but it is difficult to effectively retain the original advantages of natural fibers such as softness and high affinity. Summary of the invention
[0005] In order to solve the problems that existing synthetic fiber sponge products have better durability and cleaning ability but poor safety and softness, and natural fiber sponge products have good safety and softness but limited cleaning ability, and existing modified natural fiber sponge products also have many shortcomings, the present invention provides a sponge product and a preparation method thereof.
[0006] The main purpose of the present invention is: 1. Use natural plant fibers as raw materials to directly construct lightweight and high structural density sponge products similar to synthetic fiber sponges; Second, sponge products can maintain the safety and softness of natural fiber sponges, while having good durability and cleaning ability; 3. The preparation method is simple and efficient, and is suitable for industrial mass production.
[0007] To achieve the above objectives, the present invention adopts the following technical solutions.
[0008] A method for preparing a sponge product, The method comprises: 1) adding plant fiber into aqueous hydrogen peroxide solution to fully swell the fiber, and then filtering and separating the liquid to obtain pretreated fiber; 2) Dispersing the pretreated fibers in water, adding acrylic acid monomer, stirring and reacting until flocs are formed, then quickly adding alkali solution to adjust the pH value to 6-8 and adding water to expand the volume into a gel sponge; 3) placing the gel sponge in methanol for displacement immersion and finally performing heat drying to solidify, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge is placed in excess water for ultrasonic washing until the sponge softens, and then filtered and dried to obtain a sponge product.
[0009] As a preference, Step 1) the plant fiber is wood fiber powder and / or bamboo fiber powder with a mesh size of ≥80 mesh; Step 1) The concentration of the aqueous hydrogen peroxide solution is 25-35 wt%; In step 1), the mass ratio of the plant fiber to the aqueous hydrogen peroxide solution is 1:(2.75-3.25).
[0010] As a preference, The sufficient swelling in step 1) is carried out by swelling and immersion at 20 to 25°C for 30 to 60 minutes.
[0011] As a preference, Step 2) when dispersing the pretreated fiber into water, the mass ratio of the pretreated fiber to water is 1:(1.2-1.8); In step 2), the amount of acrylic acid monomer used is (0.8-1.2) g / g pretreated fiber.
[0012] As a preference, Step 2) the reaction temperature during the stirring reaction is controlled to be 45-55°C; Step 2) The stirring reaction time is 210 to 270 min.
[0013] As a preference, Step 2) the alkali solution is a sodium hydroxide aqueous solution with a concentration of 18 to 22 wt%; In step 2), the amount of water added for volume expansion is (20-30) mL / g pretreated fiber.
[0014] As a preference, Step 3) The heat drying solidification is carried out at 60-70°C for 2-3 hours.
[0015] As a preference, Step 4) The excess water is 3 to 5 times the volume of the solid preformed sponge.
[0016] A sponge product.
[0017] For the technical solution of the present invention, the core technology is to combine acrylic monomers with plant fibers to prepare sponge products in a similar way to modifying plant fibers. However, the difference is that the present invention is only applicable to a very small number of materials, which greatly reduces the introduction of auxiliary agents and regulators such as foaming agents and initiators, improves the safety and environmental protection of sponge products, and at the same time retains the original structural characteristics of plant fibers to a large extent, so that plant fibers maintain good flexibility and porous characteristics of the fiber surface, so as to improve the cleaning effect of sponge products.
[0018] In this regard, the present invention firstly needs to effectively pretreat the plant fibers, and the pretreatment of the present invention mainly involves treating the plant fibers with an excess of hydrogen peroxide aqueous solution at room temperature.
[0019] In this treatment process, the actual hydrogen peroxide plays a certain role as an initiator, which can make the plant fiber powder swell and expand to form filamentous fibers. At the same time, with the help of the strong oxidizing property of hydrogen peroxide, a large number of free radicals RO· are generated in the pretreatment system, thereby enabling the pretreated plant fiber to have a strong reactivity and be grafted with acrylic acid. This is also a relatively common pretreatment method used in the synthesis process of acrylic cellulose. However, for the present invention, unlike the common acrylic cellulose synthesis process which requires a pretreatment of at least 50 to 80 °C, the present invention needs to control the pretreatment temperature to be strictly within a relatively low range of 20 to 25 °C, because the use of low temperature combined with an excess of hydrogen peroxide aqueous solution can greatly improve the reactivity of the plant fiber, but can also avoid the generation of too many free radicals to stimulate the long-chain polymerization of acrylic monomers. The long-chain polymerization of acrylic monomers to form polyacrylic acid polymers with high polymerization degree and high crosslinking degree is not conducive to the preparation of the sponge product of the present invention.
[0020] This involves the second important technical point of the present invention, namely, the control of the acrylic acid polymerization process. To control the polymerization process and the properties of the polymerization product (and its derivatives, such as polyacrylic acid resin and sodium polyacrylate, etc.), the present invention firstly can directly use acrylic acid among a large number of acrylic acid monomers for free radical polymerization, because other acrylic acid monomers such as methyl methacrylate, ethyl acrylate or lauryl ester and other common acrylic acid monomers will cause the properties of the polymer to change, while the present invention needs to strictly control the crosslinking degree and polymer of the acrylic acid polymer, and these common monomers are not conducive to the control of the process.
[0021] In the reaction process between the pretreated fiber and acrylic acid of the present invention, the actual acrylic acid plays the role of "adhesive" to link the activated plant fiber with extremely strong reactivity, so that it can form a cross-linked flocculent while retaining the microstructure of the original plant fiber as much as possible, so that it maintains good affinity and flexibility to the human body. At the same time, the pretreated fiber after pretreatment also acts as an "initiator", which can promote its own grafting reaction with acrylic acid to cross-link and construct the basis of the sponge foam structure, and at the same time can stimulate acrylic acid to copolymerize to form a water-absorbent polymer, forming an interpenetrating network, and generating a supporting effect from the inside to the outside to expand the plant fiber outward to form a gel sponge with a certain hardness.
[0022] The subsequent treatment process is another important technical core of the present invention. During the research and development process, technicians found that under certain conditions, the polyacrylic acid fiber formed in the gel sponge is a polymer with very low polymerization degree and cross-linking degree, and the special polyacrylic acid fiber formed can be removed by "water washing", but before removal, it can play a good interpenetrating support role and overcome the thermal shrinkage problem of natural fiber sponge during the initial drying and curing process. Because whether it is wood fiber sponge or bamboo fiber sponge, or even higher-end bacterial cellulose sponge, it will produce irreversible volume shrinkage during the initial thermal drying process, and the thickness change rate before and after drying can even be as high as about 51-79%. This is mainly because the molecular structure of plant cellulose contains a large number of hydroxyl groups. These hydroxyl groups will form hydrogen bonds with water molecules in a wet state, making the fiber have a certain expansibility, but in the thermal drying process, the water is removed, and the hydrogen bonds between the cellulose molecular chains are rearranged, causing the molecular chains to become more compact and orderly. This structural change is irreversible, which leads to the shrinkage of the fiber sponge. Therefore, natural fiber sponges or foams need to be initially dried and solidified by freeze drying, which is costly, but this is obviously not suitable for the manufacture of cleaning sponges.
[0023] However, in the technical solution of the present invention, the plant fiber-acrylic cellulose network composed of plant fiber and acrylic acid and the polyacrylic acid fiber network form an interpenetrating support, which can inhibit the narrowing and shrinkage of the cellulose molecular chain during the heat drying process, and the surface of the polyacrylic acid fiber also contains abundant carboxyl hydroxyl groups, which can effectively stabilize the arrangement of the cellulose molecular chains through hydrogen bonding. After the initial heat drying, the plant cellulose tends to be stable, which can effectively maintain the light and flexible state of the sponge product.
[0024] Therefore, the present invention needs to ensure that in step 2), two main reaction processes, namely, grafting of plant fiber with acrylic acid and short-chain polymerization of acrylic acid, can occur. Therefore, in addition to controlling the aforementioned plant fiber pretreatment process, attention must also be paid to the reaction temperature. The present invention adopts a lower reaction temperature in order to suppress the long-chain polymerization of acrylic acid as much as possible.
[0025] After completing the initial heat drying and solidification of the gel sponge, the present invention further uses excess water for ultrasonic dissolution to achieve the "dissolution" of the low-polymerization degree and low-crosslinking degree acrylic acid polymer, so that it is converted into a low-viscosity colloid state or even almost completely dissolved, and separated from the sponge product, thereby realizing the preparation of the target sponge product.
[0026] The beneficial effects of the present invention are: The invention can realize the preparation of natural fiber sponge by combining very few raw materials and additives, and make it have the high affinity and high softness characteristics of natural sponge, while enhancing its durability and cleaning power. The preparation process is simple and efficient, and the preparation process is more green and safe. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a 20x optical microscope image of a commercial wood pulp sponge in dry form; Figure 2 This is a 20x optical microscope image of a commercial wood pulp sponge after it has absorbed water; Figure 3 This is a 20x optical microscope image of the sponge product in dry form obtained in Example 1 of the present invention; Figure 4 This is a 20x optical microscope image of the sponge product prepared in Example 1 of the present invention after absorbing water; Figure 5 This is a SEM characterization image of the sponge product prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0029] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0030] Example 1 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 1:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 22±1 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their mass, and acrylic acid of the same mass as the pretreated fibers was added. The mixture was stirred at 50 °C for 4 h to form flocs. A 20 wt% aqueous sodium hydroxide solution was quickly added within 2 min to adjust the pH value to 6.8. Pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers to expand the volume, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain a gel sponge. 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0031] Among them, the dimensions of the gel sponge, the solid prefabricated sponge and the target product sponge product were measured and recorded, and the volume shrinkage rate during the solidification process and after washing away the internal supporting acrylic polymer network during the drying process was calculated. Only the thickness is used as the standard. In this example, the average thickness of the gel sponge controlled by the cutting process in step 2) is about 3.8 cm, the average thickness of the solid prefabricated sponge obtained after thermal drying solidification is about 3.65 cm, and the average thickness of the sponge product finally obtained is about 3.58 cm. It can be seen that the natural fiber sponge product of the present invention has extremely high structural stability and will not shrink excessively due to water loss. After 100 cycles of saturated water absorption and drying, the average thickness of the sponge product is still maintained at 3.53 cm, that is, the thickness change rate is ≤1.39%. It shows very excellent structural stability and excellent durability.
[0032] In addition, during the above cycle, the present invention also performs optical microscopic characterization of the sponge in a dry state and after absorbing water (after saturated water absorption, water is squeezed out until it no longer drips, but it still feels obviously moist, the same below), and compares it with a commercially available cleaning wood pulp sponge. The optical microscopic characterization of the cleaning wood pulp sponge in a dry state is shown in FIG. Figure 1 As shown in the optical microscopy characterization of the clean wood pulp sponge after absorbing water, Figure 2 As shown, from Figure 1 and Figure 2 By comparison, it can be clearly seen that the commercially available wood pulp sponge has undergone very obvious structural changes in the dry state and after absorbing water. After absorbing water, the plant fiber obviously "expands" due to hydrogen bonding, but shrinks after drying and losing water. This will inevitably cause structural collapse during use. For example, in the same saturated water absorption and drying cycle test, the commercially available cleaning wood pulp sponge has a thickness change rate of about 8.3% after 80 cycles. This thickness change is irreversible. The optical microscopic characterization diagrams of the sponge product of the present invention in the dry state and after absorbing water are shown in Figure 2. Figure 3 and Figure 4 As shown in the figure, the structure of the sponge product in the dry state and after absorbing water has hardly changed, which also shows that it has extremely high structural stability. The results of the water absorption-drying cycle test also show that the sponge product of the present invention has extremely strong durability. In addition, the sponge product prepared in this example was characterized by electron microscopy, and the structure was characterized as shown in the figure. Figure 5 As shown, from Figure 5 It can be clearly seen that the fibers of the sponge product of the present invention maintain the surface porosity of natural plant fibers, which makes it have super high water absorption that synthetic fibers do not have. It also shows that although the preparation process of the present invention seems to be similar to the preparation process of modified cellulose, it still retains the structure of the plant fiber itself to a large extent, which ensures that it has good affinity and water absorption.
[0033] Based on the above, the common properties of sponge products are characterized and compared with commercially available wood pulp sponges and synthetic fiber sponges. The sponges used for comparison are all of the same size. The characterization results are shown in the following table.
[0034] Table 1: Performance criteria results.
[0035] In the table: Due to the dry and hardened characteristics of wood pulp sponge, the tensile strength and elongation at break are tested under water absorption; the thousand-times wear rate is measured by soaking one side of the sponge to be tested in pure water, placing the soaked wetted surface on a platform of the same material (304 stainless steel platform), pressing a 3 kg counterweight, and rubbing it back and forth 1000 times at the same rate. The single friction distance is 10 cm. The mass before and after friction is measured and recorded, and the mass loss rate after friction is calculated and recorded as the thousand-times wear rate.
[0036] It can be clearly seen from the above characterization results that the sponge product of the present invention has a lower density than the commercially available wood pulp sponge, and has obvious low-density characteristics, while the tensile strength and elongation at break are significantly better than the commercially available wood pulp sponge, that is, the natural fiber sponge, and close to the synthetic fiber sponge, and the difference between the dry hardness and the water absorption hardness is small, and the water absorption hardness is much higher than the commercially available wood pulp sponge, which is already close to the commercially available synthetic fiber sponge, which makes it have very excellent cleaning ability, because the sponge hardness after water absorption is a key parameter that determines its cleaning ability. As for the previous wear rate, due to the flexibility of the natural plant fiber itself, its wear rate is also much lower than that of the synthetic fiber sponge, which is similar to the commercially available wood pulp sponge, and the wear and tear is not the plastic component of the synthetic fiber sponge, but a safer natural fiber component, which makes the sponge product of the present invention also have extremely high safety of use.
[0037] Example 2 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 2:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 22±1 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their mass, and acrylic acid of the same mass as the pretreated fibers was added. The mixture was stirred at 50 °C for 4 h to form flocs. A 20 wt% aqueous sodium hydroxide solution was quickly added within 2 min to adjust the pH value to 7.0. Pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers to expand the volume, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain a gel sponge. 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0038] The sponge product prepared in this example was characterized in the same manner as in Example 1. The characterization results are shown in the following table.
[0039] Table 2: Performance criteria results.
[0040] It can be clearly seen from the above characterization results that the sponge product prepared in this example also has good performance, good durability and cleaning ability, and at the same time has the safety of natural fiber sponge.
[0041] Comparative Example 1 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 1:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 55±1.5 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their mass, and acrylic acid of the same mass as the pretreated fibers was added. The mixture was stirred at 50 °C for 4 h to form flocs. A 20 wt% aqueous sodium hydroxide solution was quickly added within 2 min to adjust the pH value to 6.8. Pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers to expand the volume, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain a gel sponge. 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0042] The sponge product prepared in this example was characterized in the same manner as in Example 1. The characterization results are shown in the following table.
[0043] Table 3: Performance criteria results.
[0044] From the above characterization results, compared with Example 1, almost all properties except the wear rate per thousand times are improved in this example, but this is actually not what the present invention requires. Because in the product prepared in this example, the mass ratio of the product mass to the plant fiber used (the total mass of wood fiber powder and bamboo fiber powder) is about 1.37:1, while the mass ratio of the product mass to the plant fiber used (the total mass of wood fiber powder and bamboo fiber powder) in Example 1 is about 1.09:1, it can be seen that the sponge product prepared in this example contains a large amount of acrylic acid polymer and its derivatives, which does not meet the purpose of the present invention to prepare a natural fiber sponge with high safety and green environmental protection, and its wear rate per thousand times is also significantly improved, which also shows that it contains more synthetic fiber components that are easy to wear and fall off.
[0045] This is mainly because the excessively high pretreatment temperature causes the pretreated fiber to form more free radicals, which leads to the formation of long-chain polymerization of acrylic acid and a higher degree of crosslinking, making it more difficult to remove in the subsequent "water washing" process, or even impossible to remove. This does not conform to the original intention of the present invention.
[0046] Comparative Example 2 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 1:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 22±1 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their mass, and acrylic acid monomer (acrylic acid and lauryl methacrylate were mixed in a mass ratio of 1:0.1) of the pretreated fibers was added, and stirred at 50 °C for 4 h to form flocs, and then a 20 wt% sodium hydroxide aqueous solution was quickly added within 2 min to adjust the pH value to 6.8, and pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers for volume expansion, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain gel sponges; 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0047] The sponge product prepared in this example was characterized in the same manner as in Example 1. The characterization results are shown in the following table.
[0048] Table 4: Performance criteria results.
[0049] It can be clearly seen from the above characterization results that the sponge product prepared in this example is similar to the product of Comparative Example 1, and its performance is actually better than that of the product of Example 1 in many aspects. However, similarly, the mass ratio of its product mass to the mass of the plant fiber used (total mass of wood fiber powder and bamboo fiber powder) is about 1.41:1, which is even higher than that of Comparative Example 1. This is mainly due to the use of lauryl methacrylate as one of the monomers in this example, which significantly improves the water resistance of acrylic polymers and their derivatives, making them difficult to remove by washing, and also leaving more synthetic fiber components, which does not meet the original intention of the research and development of the present invention.
[0050] Comparative Example 3 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 1:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 22±1 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their mass, and acrylic acid of the same mass as the pretreated fibers was added. The mixture was stirred at 65 °C for 4 h to form flocs. A 20 wt% aqueous sodium hydroxide solution was quickly added within 2 min to adjust the pH value to 6.8. Pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers to expand the volume, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain a gel sponge. 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0051] The sponge product prepared in this example was characterized in the same manner as in Example 1. The characterization results are shown in the following table.
[0052] Table 5: Performance criteria results.
[0053] It can be clearly seen from the above characterization results that the sponge product prepared in this example is similar to the products of Comparative Examples 1 and 2, and its performance in many properties is actually close to or even better than the product of Example 1, but similarly, the mass ratio of its product mass to the mass of the plant fiber used (total mass of wood fiber powder and bamboo fiber powder) is about 1.18:1, which is much higher than that of Example 1. This is mainly due to the use of a higher free radical polymerization reaction temperature in this example, which increases the chain length and polymer of the acrylic acid polymer and its derivatives, making it difficult to wash and remove, and also leaves more synthetic fiber components, which does not meet the original intention of the research and development of the present invention.
[0054] Comparative Example 4 A method for preparing a sponge product, The method comprises: 1) 80 mesh wood fiber powder and 120 mesh bamboo fiber powder were mixed in a mass ratio of 1:1, added into a 30 wt% hydrogen peroxide aqueous solution, fully immersed and swollen at 22±1 ℃ for 50 min, and then the liquid was separated by filtration to obtain pretreated fiber; 2) The pretreated fibers were dispersed in pure water 1.5 times their weight, and acrylic acid 0.2 times the weight of the pretreated fibers was added. The mixture was stirred at 50 °C for 4 h to form flocs. A 20 wt% sodium hydroxide aqueous solution was quickly added within 2 min to adjust the pH value to 6.8. Pure water was added at a ratio of 25 mL of pure water per gram of pretreated fibers to expand the volume, and the pretreated fibers were cut into block-shaped rectangular blocks to obtain a gel sponge. 3) The gel sponge was immersed in anhydrous methanol and ultrasonically treated for 15 min to perform solvent replacement and washing, and finally, it was thermally dried at 65°C for 2.5 h to complete solidification, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge was placed in pure water with a volume 5 times its own for ultrasonic immersion for 60 min. The ultrasonic immersion was repeated 3 times until the sponge was completely softened, and then filtered and dried at 60 °C for 12 min to obtain a sponge product.
[0055] The sponge product prepared in this example was characterized in the same manner as in Example 1. The characterization results are shown in the following table.
[0056] Table 6: Performance criteria results.
[0057] It can be clearly seen from the above characterization results that the sponge product prepared in this example exhibits performance more similar to that of a wood pulp sponge, with density and tensile strength increased compared to Example 1, and elongation at break decreased compared to Example 1, while the difference between dry hardness and water absorption hardness is large, with obvious drying and hardening phenomenon. This is mainly because the present invention uses less acrylic acid monomer, which can only play the role of "adhesive", and the mass ratio of its product mass to the mass of the plant fiber (total mass of wood fiber powder and bamboo fiber powder) used is about 1.08:1, which is close to Example 1. In the preparation process, the average thickness of the gel sponge controlled by the cutting process in step 2) of this example is about 3.8 cm, and the average thickness of the solid prefabricated sponge obtained after heat drying and solidification is about 3.01 cm, while the average thickness of the sponge product finally obtained is about 2.93 cm, and the thickness shrinkage rate is much higher than that of Example 1, reaching about 22.9%. Combined with the aforementioned comparative examples 1 to 3, it can be clearly seen that the present invention adopts the form of using an appropriate amount of acrylic acid and controlling it to perform appropriate polymerization, which can play a supporting role in the heat drying and solidification process. At the same time, the polymer and its derivatives formed under appropriate polymerization conditions can be easily washed and removed, so as to ensure that the sponge product of the present invention has the characteristics similar to natural fiber sponge, but has better performance.
Claims
1. A method for preparing a sponge product, characterized in that: The method comprises: 1) adding plant fiber into aqueous hydrogen peroxide solution to fully swell the fiber, and then filtering and separating the liquid to obtain pretreated fiber; 2) Dispersing the pretreated fibers in water, adding acrylic acid monomer, stirring and reacting until flocs are formed, then quickly adding alkali solution to adjust the pH value to 6-8 and adding water to expand the volume into a gel sponge; 3) placing the gel sponge in methanol for displacement immersion and finally performing heat drying to solidify, thereby obtaining a solid prefabricated sponge; 4) The solid prefabricated sponge is placed in excess water for ultrasonic washing until the sponge softens, and then filtered and dried to obtain a sponge product.
2. The method for preparing a sponge product according to claim 1, characterized in that: Step 1) the plant fiber is wood fiber powder and / or bamboo fiber powder with a mesh size of ≥80 mesh; Step 1) The concentration of the aqueous hydrogen peroxide solution is 25-35 wt%; In step 1), the mass ratio of the plant fiber to the aqueous hydrogen peroxide solution is 1:(2.75-3.25).
3. The method for preparing a sponge product according to claim 1 or 2, characterized in that: The sufficient swelling in step 1) is carried out by swelling and immersion at 20 to 25°C for 30 to 60 minutes.
4. The method for preparing a sponge product according to claim 1, characterized in that: Step 2) when dispersing the pretreated fiber into water, the mass ratio of the pretreated fiber to water is 1:(1.2-1.8); In step 2), the amount of acrylic acid monomer used is (0.8-1.2) g / g pretreated fiber.
5. The method for preparing a sponge product according to claim 1 or 4, characterized in that: Step 2) the reaction temperature during the stirring reaction is controlled to be 45-55°C; Step 2) The stirring reaction time is 210 to 270 min.
6. The method for preparing a sponge product according to claim 1, characterized in that: Step 2) the alkali solution is a sodium hydroxide aqueous solution with a concentration of 18 to 22 wt%; In step 2), the amount of water added for volume expansion is (20-30) mL / g pretreated fiber.
7. The method for preparing a sponge product according to claim 1, characterized in that: Step 3) The heat drying solidification is carried out at 60-70°C for 2-3 hours.
8. The method for preparing a sponge product according to claim 1, characterized in that: Step 4) The excess water is 3 to 5 times the volume of the solid preformed sponge.
9. A sponge product obtained by the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparation method of cellulose-based water absorbent material
CN102382264A
Preparation method of high-purity sponge spicules
CN105858669A
Preparation method of rapid absorption type super absorbent resin
CN108610459A
Plant-derived aerogels, hydrogels, and foams, methods and uses thereof
CN116322363A
Bagasse cellulose grafted polyacrylic acid hydrogel as well as preparation method and application thereof