Method for low-temperature decoking and surface activation of pyrolyzed and recycled carbon fibers

Through low-temperature ozone oxidation and semi-coke removal and surface activation technology, the problems of fiber cleanliness and strength in pyrolytic recovery of carbon fibers are solved, and efficient and low-energy-consuming fiber recovery and composite performance improvement are achieved.

CN119019757APending Publication Date: 2024-11-26SHANGHAI TANJI IND GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411112962.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing methods of pyrolysis recovery of carbon fibers during high-temperature oxidation lead to incomplete removal of semi-coke adhesion on the fiber surface, resulting in low cleanliness of recovered fibers and reduced composite strength, high additional energy consumption and difficult to control.

Method used

The high-efficiency oxidation of low-temperature ozone is used to remove semi-cokes and activate the carbon fiber surface. It is pretreated by impregnation of zinc acetate ethanol solution. After pyrolysis, air oxidation is introduced at 450-550℃, and then ozone is introduced at 90-180℃ for surface activation. Reduce additional oxidation processes and improve fiber cleanliness and strength.

Benefits of technology

Remove more than 50% of semi-cokes in the range of 200-550°C, and the low-temperature ozone treatment can remove 99.9% semi-cokes, reducing energy consumption, retaining fiber strength by 10% higher than conventional oxidation operations, and improving the adhesion between the fiber and the resin matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992815980000061
    Figure BDA0004992815980000061
  • Figure BDA0004992815980000071
    Figure BDA0004992815980000071
Patent Text Reader

Abstract

The invention discloses a method for low-temperature decoking and surface activation of pyrolyzed and recycled carbon fibers, which comprises the following steps: dipping a carbon fiber reinforced composite material in an ethanol solution of zinc acetate, cleaning and drying after dipping, and then performing high-temperature pyrolysis in an inert atmosphere; after the pyrolysis is finished, introducing air, and carrying out in-situ oxidation along with the furnace so as to remove semicoke; after in-situ oxidation along with the furnace reaches a certain temperature, air introduction is stopped, ozone is introduced to enhance decoking and perform surface activation, and after the surface activation is finished, cleaning and drying are performed to prepare the recycled fibers. According to the method, ozone is introduced at the temperature of 200 DEG C or below, and 99.9% or above of semicoke can be removed; compared with conventional air oxidation at constant temperature, the expected energy consumption is greatly reduced; the oxygen-containing functional group comparison index O / C of the recycled fiber and the fresh fiber is maintained above 80%; and the fiber strength retention after ozone oxidation treatment at 200 DEG C or below is 10% or above higher than that of the conventional oxidation operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recycling fibers, in particular to a method for pyrolysis recycling of carbon fibers, low-temperature decoking and surface activation. Background Art

[0002] Carbon fiber reinforced resin-based composite materials are formed by curing the reinforcement carbon fiber and the resin matrix. Usually, thermoplastic resins have thermal reprocessability, while a large number of thermosetting resin-based composite materials cannot be reversed by heating due to their molecular cross-linked structure. Therefore, the investment cost is low, the fiber retains high strength, and the environmentally friendly and energy-saving pyrolysis method is widely used in the degradation and recycling of carbon fiber reinforced composite materials.

[0003] As an incomplete thermochemical conversion technology, pyrolysis is usually carried out in an inert atmosphere at 300-800°C, which converts the resin into small volatile molecules and retains the carbon fiber. However, the pyrolysis of the resin matrix is ​​also accompanied by the generation of a certain amount of semi-coke, which will adhere to the fiber surface, resulting in low surface cleanliness of the recycled carbon fiber. The subsequent poor interface with the resin further leads to low strength of the prepared composite material.

[0004] Currently, CN103665430A, CN107216480A, and CN104262675A use oxygen-containing atmosphere pyrolysis to recycle carbon fiber, but the cleanliness of the recycled fiber is not enough. Since then, the pyrolysis recovery process of carbon fiber composites has evolved into a two-step method. The first step is the pyrolysis of the resin matrix, mainly to degrade the resin matrix as much as possible. The second step is the oxidation removal of the semi-coke at a higher temperature, and the oxidizing medium is introduced to remove the residual semi-coke and silane coupling agent generated by the pyrolysis of the resin matrix. The specific forms are: ① in-situ oxidation CN106957451B, US20200002619A1, CN108610507A, US11319489B2; ② non-in-situ oxidation: EP3023478B1, EP3023478A2, EP3023478A3, CN108690218A, US10072358B2, US20160153123A1; ③ oxidation in reaction intervals: US10899042B2, US20190039266A1, EP3444091A1, US10723954B2, US20190248045A1, US11331831B2. Usually, the air oxidation process is above 400°C, which increases the extra energy consumption and the reaction is intense and difficult to control. Although the attached semi-coke can be removed as much as possible, it is also accompanied by deep oxidation, which causes the carbon fiber to lose weight, increase defect sites, and greatly reduce strength.

[0005] Currently, the gas phase oxidation process of the recycled fiber mentioned in the above patent is easy to operate and has significant effects, but the activation of the surface of the recycled fiber is not implemented. Summary of the invention

[0006] Purpose of the invention: The purpose of the present invention is to provide a method for low-temperature decoking and surface activation of carbon fibers by using highly active ozone to efficiently oxidize and remove semi-coke at low temperatures and activate the carbon fiber surface by pyrolysis recovery.

[0007] Technical solution: The method for low-temperature decoking and surface activation of pyrolysis-recovered carbon fiber of the present invention comprises the following steps:

[0008] (1) immersing the carbon fiber reinforced composite material in an ethanol solution of zinc acetate, and washing and drying after the immersion is completed;

[0009] (2) subjecting the dried carbon fiber reinforced composite material to high temperature pyrolysis in an inert atmosphere;

[0010] (3) After the pyrolysis is completed, air is introduced to oxidize in situ in the furnace to remove the semi-coke;

[0011] (4) After the in-situ oxidation in the furnace, the air supply is stopped and ozone is introduced to enhance the decoking and surface activation. After completion, the fiber is cleaned and dried to obtain the recycled fiber.

[0012] Wherein, in step (1), the concentration of the zinc acetate ethanol solution is 2.5 to 3.5 mol / L.

[0013] Wherein, in step (2), pyrolysis is carried out at a temperature of 450-550° C. for 30-60 min.

[0014] Wherein, in step (2), the inert atmosphere is a nitrogen atmosphere; and the flow rate of the inert atmosphere is 100 to 300 mL / min.

[0015] Wherein, in step (3), air is introduced at a temperature of 450-550°C.

[0016] Wherein, in step (3), the flow rate of the incoming air is maintained at a furnace cooling rate of 5-15°C / min.

[0017] In step (4), the concentration of ozone introduced is 1-10 mg / L, more preferably 1.5-5.0 mg / L. Ozone of appropriate concentration can effectively increase the content of oxygen-containing functional groups on the surface of the recycled carbon fiber. If the concentration is too low, the oxidation activity is insufficient. If the concentration is too high, the oxidation activity is too strong, which can easily cause damage to the surface of the recycled fiber, such as pits and holes. Ozone is introduced at a temperature of 90°C-180°C, and the time of ozone introduction is 2.5-5 minutes.

[0018] Wherein, in step (4), when the furnace temperature drops to 90-180° C., the introduction of air is stopped and then ozone is introduced.

[0019] Principle of invention: Ozone is a strong oxidant that can react with carbon atoms on the surface of carbon fiber to increase surface functional groups, especially carbonyl functional groups. The oxidation reaction causes a change in the degree of graphitization of the carbon fiber surface, increases the surface roughness, and thus improves the wettability of the carbon fiber, which helps to improve the bonding between the fiber and the resin matrix, reduce the formation of traps in the composite material, and thus improve the strength of the composite material. Considering that ozone has high oxidation activity at high temperatures, but has a short stable existence time above 200°C, and has poor low-temperature reaction activity, 90-180°C is generally selected. Pretreatment by impregnation with zinc acetate ethanol solution to achieve a loose pore structure of pyrolysis semi-coke, which is conducive to the diffusion of air and ozone; cooling with the furnace, using air for partial oxidation to remove semi-coke above 200°C, reducing the ozone decoking load below 200°C, and recycling carbon fiber cleaner; using ozone to efficiently decoke below 200°C, and oxidatively activate the carbon fiber surface, making full use of heat, and reducing an additional oxidation activation process.

[0020] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects: (1) Air is introduced during the high temperature stage of the furnace cooling process at 200-550°C to remove more than 50% of the attached semi-coke; (2) Ozone is introduced during the low temperature stage below 200°C to further eliminate the above-mentioned semi-coke oxidized in the furnace, and it is expected that more than 99.9% of the semi-coke can be removed; (3) Compared with constant temperature air oxidation under conventional high temperature conditions, it is expected that energy consumption will be greatly reduced; (4) When ozone is introduced below 200°C, the oxygen-containing functional group comparison index O / C of the recycled fiber and the fresh fiber is maintained at more than 80%; (5) The fiber strength retention after ozone oxidation treatment below 200°C is more than 10% higher than that of conventional oxidation operation. DETAILED DESCRIPTION

[0021] The present invention is described in further detail below.

[0022] Example 1

[0023] The carbon fiber reinforced composite materials used in the embodiments and comparative examples of the present invention are the same, wherein the carbon fiber is Toray T700s and the resin matrix is ​​bisphenol A epoxy resin.

[0024] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0025] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the flow rate of the air was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 150°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0026] Example 2

[0027] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0028] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The gas velocity was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 130°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0029] Example 3

[0030] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0031] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The gas velocity was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 130°C, an oxidizing atmosphere with an O3 content of 4 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0032] Example 4

[0033] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0034] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The gas velocity was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 180°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0035] Example 5

[0036] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0037] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 110°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0038] Example 6

[0039] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0040] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 2.5 mol / l zinc acetate ethanol solution, and ultrasonicated for 2h; washed with deionized water and dried at 60℃ for 24h under normal pressure. Heated to 550℃, nitrogen was introduced at a flow rate of 100ml / min, pyrolyzed for 30min, and heating was stopped and switched to air. The air flow rate was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 5℃ / min; when the furnace temperature dropped to about 110℃, an oxidizing atmosphere with an O3 content of 2.5mg / L was introduced until the furnace temperature dropped to 90℃, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0041] Example 7

[0042] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0043] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3.5 mol / l zinc acetate ethanol solution, and ultrasonicated for 2h; washed with deionized water and dried at 60℃ for 24h under normal pressure. Heated to 550℃, nitrogen was introduced at a flow rate of 200ml / min, pyrolyzed for 60min, and heating was stopped and switched to air. The air flow rate was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 15℃ / min; when the furnace temperature dropped to about 110℃, an oxidizing atmosphere with an O3 content of 2.5mg / L was introduced until the furnace temperature dropped to 90℃, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0044] Comparative Example 1

[0045] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0046] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0047] Comparative Example 2

[0048] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0049] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, and pyrolysis was performed for 30 minutes. The temperature was kept at 500°C, switched to air and kept warm for 15 minutes. Then the heating was stopped, and the air flow rate was adjusted so that the air flow rate was maintained at a furnace cooling rate of about 10°C / min; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0050] Comparative Example 3

[0051] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0052] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, and pyrolysis was performed for 30 minutes. The temperature was quickly raised to 550°C, switched to air and kept warm for 15 minutes. Then the heating was stopped and the air flow rate was adjusted so that the air flow rate was maintained at a cooling rate of about 10°C / min in the furnace; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0053] Comparative Example 4

[0054] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0055] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60℃ for 24 hours under normal pressure. Heated to 450℃, nitrogen was introduced at a flow rate of 300ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the flow rate of the air was maintained at a furnace cooling rate of about 10℃ / min; when the furnace temperature dropped to about 150℃, an oxidizing atmosphere with an O3 content of 10mg / L was introduced until the furnace temperature dropped to 90℃, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0056] Comparative Example 5

[0057] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0058] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the flow rate of the air was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 150°C, an oxidizing atmosphere with an O3 content of 1 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0059] Comparative Example 6

[0060] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0061] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the flow rate of the air was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 250°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 90°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0062] Comparative Example 7

[0063] A method for pyrolysis recovery of carbon fiber, low temperature decoking and surface activation, comprising the following steps:

[0064] The carbon fiber reinforced composite material was cut into 10x10 cm, immersed in 3 mol / l zinc acetate ethanol solution, and ultrasonicated for 2 hours; washed with deionized water and dried at 60°C for 24 hours under normal pressure. Heated to 450°C, nitrogen was introduced at a flow rate of 300 ml / min, pyrolyzed for 30 minutes, and heating was stopped and switched to air. The air flow rate was adjusted so that the flow rate of the air was maintained at a furnace cooling rate of about 10°C / min; when the furnace temperature dropped to about 90°C, an oxidizing atmosphere with an O3 content of 2.5 mg / L was introduced until the furnace temperature dropped to 70°C, and then switched to nitrogen; after the furnace temperature dropped to room temperature, the material was taken out, washed with water, and dried to obtain recycled fiber.

[0065] The fresh carbon fiber of Toray T700s and the fibers obtained in the above embodiments and comparative examples were characterized and tested, and the results are shown in Table 1 below.

[0066] Table 1

[0067]

[0068]

Claims

1. A method for low-temperature decoking and surface activation of pyrolytically recovered carbon fibers, characterized in that: The following steps are involved: (1) immersing the carbon fiber reinforced composite material in an ethanol solution of zinc acetate, and washing and drying after the immersion is completed; (2) subjecting the dried carbon fiber reinforced composite material to high temperature pyrolysis in an inert atmosphere; (3) After the pyrolysis is completed, air is introduced to oxidize in situ in the furnace to remove the semi-coke; (4) After the in-situ oxidation in the furnace, the air supply is stopped and ozone is introduced to enhance the decoking and surface activation. After completion, the fiber is cleaned and dried to obtain the recycled fiber.

2. The method for low-temperature decoking and surface activation of pyrolysis-recovered carbon fiber according to claim 1, characterized in that: In step (4), the concentration of ozone introduced is 1-10 mg / L.

3. The method for low-temperature decoking and surface activation of pyrolysis-recovered carbon fiber according to claim 1, characterized in that: In step (4), ozone is introduced at a temperature of 90-180° C. for a period of 2.5-5 minutes.

4. The method for low-temperature decoking and surface activation of pyrolysis-recovered carbon fiber according to claim 1, characterized in that: In step (4), when the furnace temperature drops to 90-180° C., the air supply is stopped.

5. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (1), the concentration of the zinc acetate ethanol solution is 2.5-3.5 mol / L.

6. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (2), pyrolysis is performed at 450-550° C. for 30-60 min.

7. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (3), air is introduced at a temperature of 450-550°C.

8. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (3), the flow rate of the air is maintained at a furnace cooling rate of 5-15°C / min.

9. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (2), the inert atmosphere is a nitrogen atmosphere.

10. The method for low-temperature decoking and surface activation of pyrolytically recovered carbon fiber according to claim 1, characterized in that: In step (2), the flow rate of the inert atmosphere is 100 to 300 ml / min.

Citation Information

Cited By

  • Preparation method of BMC composite material based on pyrolysis recovery of carbon fibers

    CN121270973A