Non-transparent film agent for replacing titanium dioxide and preparation method of non-transparent film agent

By combining water-soluble sugars or sugar alcohols with starch, combined with surfactants, a white opaque film is formed, which solves the problem of carcinogenic risk of titanium dioxide and achieves a safe and efficient white opaque effect and long-term stability.

CN119019762APending Publication Date: 2024-11-26SHANGHAI MODERN PHARMACEUTICAL ENGINEERING RESEARCH CENTER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226226.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, titanium dioxide as an opaque agent has a risk of carcinogenic substances, which may be banned in Europe, and its substitutes such as calcium carbonate, zinc oxide and talc cannot effectively replace their whiteness and opacity.

Method used

Use water-soluble sugars or combinations of sugar alcohols and starch as opaque materials. By controlling the starch particle size and the ratio of water-soluble sugars or sugar alcohols, a white opaque film is formed to replace titanium dioxide, and promote crystallization through surfactants to improve Mechanical properties and stability of film agents.

Benefits of technology

It achieves a safe and efficient white opacity effect, and the white opacity is stable for a long time and is not easy to fall off. It has excellent melting performance, solving the problem that titanium dioxide substitutes are difficult to replace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides an opaque film agent for replacing titanium dioxide and a preparation method thereof, and the opaque film agent is mainly prepared from the following raw materials by mass: 20-80% of a polymer film-forming material; 10%-40% of water-soluble sugar or water-soluble sugar alcohol; 1%-5% of starch; 0.5%-2% of a surfactant; 0%-50% of an active component; wherein the particle size of the starch is 1-50 [mu] m. According to the film agent, the combination of the starch and the water-soluble saccharide or sugar alcohol is utilized, so that the film has a white and non-transparent appearance, a feasible solution technology is provided for replacing titanium dioxide in a film agent prescription, and the safety is improved; meanwhile, the white color can be stable for a long time and cannot fall off from the surface, and the film agent has excellent melting performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pharmaceutical preparations, and in particular to an opaque film agent replacing titanium dioxide and a preparation method thereof. Background Art

[0002] Film is a thin film preparation with the characteristics of convenient administration, simple process and good compliance. In recent years, it has received extensive attention from the food, medicine and other industries. Films usually need to be treated with opacity and coloring to give them a good appearance and improve recognition, which is especially important for children and the elderly with poor eyesight. In addition, in films containing ingredients that are easily affected by light, adding white opaque agents can also be used to block light and improve product quality. At present, the most commonly used white opaque colorant on the market is titanium dioxide, which has excellent whiteness, opacity, colorability and extremely high chemical stability. It has been widely used in the fields of food, medicine, health products and cosmetics for a long time. Due to its inherent characteristics and finer particle size, it can achieve good light-shielding and coloring effects even at lower usage levels. Titanium dioxide can be used alone or in combination with other pigments or pigments such as ferric oxide to obtain bright colors and further enhance recognizability and aesthetics.

[0003] However, in recent years, the safety of titanium dioxide has been questioned. In 2016, the French authorities submitted a proposal to the European Chemicals Agency (ECHA) to list titanium dioxide as a carcinogen. Subsequently, the Assessment Committee (RAC) passed a resolution to classify titanium dioxide as a Category 2 carcinogen the following year. In May 2021, based on concerns about the safety of "nanoscale materials", the European Food Safety Authority believed that the genotoxicity of titanium dioxide could not be ruled out; from August 7, 2022, the EU completely banned titanium dioxide as a food additive. In the same year, the European Medicines Agency issued a Q&A, calling on pharmaceutical companies to "make every possible effort" to speed up the research and development of titanium dioxide alternatives, because titanium dioxide may be banned from use in medicines in Europe within the next three years.

[0004] Currently, there are few research reports on titanium dioxide replacement. A few researchers have tried to replace titanium dioxide with white materials such as calcium carbonate, zinc oxide and talc, but the results show that the whiteness and opacity provided by these materials are weaker than titanium dioxide. In addition, these insoluble materials may also have a large number of 1nm-100nm particles, and there is also the toxicity risk of nano-scale particles.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide an opaque film that can replace titanium dioxide. The present invention uses a film of water-soluble sugars or sugar alcohols and starch to replace titanium dioxide as the opaque material of the film. During the process of making the film and drying it, the film gradually turns white, which can effectively replace titanium dioxide and has high safety. The white color can be stable for a long time without falling off the surface, and the film has excellent solubility properties.

[0007] The second object of the present invention is to provide a method for preparing the above-mentioned opaque film agent that replaces titanium dioxide, which can make it easier for crystals on the surface of the film to precipitate and form a white opaque effect.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides an opaque film agent that replaces titanium dioxide, which is mainly prepared from the following raw materials in terms of mass percentage: Polymer film-forming materials 20%-80%; Water-soluble sugars or water-soluble sugar alcohols 10%-40%; Starch 1%-5%; Surfactant 0.5%-2%; Active ingredient 0%-50%; Wherein, the particle size of the starch is 1 μm-50 μm.

[0009] The mass percentage of the polymer film-forming material may also be 30%, 40%, 50%, 60% or 70%; The mass percentage of water-soluble sugars or water-soluble sugar alcohols can also be 20% or 30%; The mass percentage of starch can also be 2%, 3% or 4%; The mass percentage of the surfactant can also be 1% or 1.5%; The mass percentage of active ingredients can also be 10%, 20%, 30% or 40%; It also includes other ingredients and other auxiliary materials 0%-30%; Other auxiliary materials may include one or more of disintegrants, plasticizers, stabilizers, colorants and flavoring agents; the mass percentage may also be 10%, 15%, 20%, 25%, 30%.

[0010] The polymer film-forming material includes one or more of hydroxypropyl methylcellulose, polyvinyl alcohol, hydroxypropyl cellulose, hydroxyethyl cellulose, polyvinyl pyrrolidone, polyvinyl alcohol-polyethylene glycol graft copolymer, maltodextrin, polyethylene oxide, sodium alginate, hydroxypropyl starch and carbomer; preferably, the auxiliary film-forming material is one or more of hydroxypropyl methylcellulose, polyvinyl alcohol, hydroxypropyl cellulose.

[0011] The water-soluble sugar or sugar alcohol includes one or more of sucrose, maltose, fructose, glucose, lactose, trehalose, mannitol, xylitol, maltitol, lactitol and erythritol; preferably, the water-soluble sugar or sugar alcohol is one or more of sucrose, trehalose, fructose and maltitol.

[0012] The surfactant includes one or more of sodium lauryl sulfate, Tween, poloxamer, lecithin, sucrose fatty acid ester, polyoxyethylene oleyl alcohol ether and stearic acid glyceryl ester; preferably, the surfactant is one or more of sucrose fatty acid ester, polyoxyethylene oleyl alcohol ether and stearic acid glyceryl ester.

[0013] The active ingredients include one or more of drugs, health functional factors and food ingredients.

[0014] In the present invention, when the proportion of water-soluble sugars or water-soluble sugar alcohols is in the range of 10%-40%, the whiteness or opacity of the film can solve the technical problem actually to be solved by the present invention. When the proportion exceeds 40%, the corresponding film-forming material is too little, and the film agent becomes brittle and easily broken; when the proportion is lower than 10%, the film will not turn completely white, and the ideal light-shielding or opaque effect cannot be achieved.

[0015] In the present invention, starch and water-soluble sugars or water-soluble sugar alcohols are added to the film-forming material, and the film gradually becomes white during the drying process of the film agent. Usually, the particle size of starch is between 1 μm and 50 μm. The particle size of starch will affect the crystallization effect of starch. When the particle size of starch is too large, the film-forming surface is rough and the white crystals are uneven; when the particle size of starch is too small, it is not conducive to the formation of crystal seeds, which will affect the whiteness of the subsequent film.

[0016] Preferably, as a further specific embodiment, the particle size of the starch is 2 μm-20 μm; Preferably, the starch has a particle size of 15 μm.

[0017] Preferably, when the starch particle size is maintained between 2 μm and 20 μm, the surface of the starch is smooth, which can promote the formation of crystal seeds; and more preferably, when the starch particle size is 15 μm, the starch can better interact with water-soluble sugars or water-soluble sugar alcohols and surfactants, so that the prepared film presents a white and opaque appearance, and the appearance of the film is better, which can solve the technical problem proposed by the present invention.

[0018] Since the amount of water-soluble sugar or water-soluble sugar alcohol used in the present invention is 10%-40%, and the amount of surfactant used is 0.5%-2%, the theoretical range of the mass ratio of water-soluble sugar or water-soluble sugar alcohol to surfactant in the present invention is (5:1)-(80:1); in actual use, the mass ratio of water-soluble sugar or water-soluble sugar alcohol to surfactant is (1:1)-(40:1).

[0019] Preferably, as a further specific embodiment, the mass ratio of the water-soluble sugar or water-soluble sugar alcohol to the surfactant is (10:1)-(20:1); The mass ratio may also be 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1 or 18:1.

[0020] Preferably, the mass ratio of the water-soluble sugar or water-soluble sugar alcohol to the surfactant is 19:1.

[0021] In the present invention, in the process of preparing the film, water-soluble sugars or water-soluble sugar alcohols and surfactants will form microcrystals during the preparation process. In addition to starch itself, which helps the formation or growth of crystals; hydrogen bonds will be formed between the hydrophilic groups of the surfactant and the water-soluble film-forming material, reducing the surface tension, thereby reducing the viscosity of the slurry, making it easy for sugars or sugar alcohols to diffuse and crystallize. At the same time, the repulsive force of the surfactant on water molecules is greater than the attractive force, which will accelerate the evaporation of water, thereby allowing crystals to form quickly. Therefore, the mass ratio of water-soluble sugars or water-soluble sugar alcohols to surfactants will also ultimately affect the morphology of film formation by affecting the microcrystals. Therefore, the ratio between water-soluble sugars or water-soluble sugar alcohols and surfactants is usually between (1:1) and (40:1), and the preferred mass ratio is (10:1) to (20:1). When the surfactant ratio is too low, the slurry viscosity is too high, the crystallization is uneven, and the speed is slow. When the film is just dry, it still cannot be completely crystallized. If it is over-dried, it is easy to break, affecting the mechanical properties of the film. When the surfactant ratio is too high, the surface interface energy of the crystalline material is reduced, the formation of crystal seeds is inhibited, and it is difficult to crystallize.

[0022] The more preferred mass ratio of water-soluble sugars or water-soluble sugar alcohols to surfactants is 19:1, which is the optimal ratio of the two and can ensure complete crystallization and rapid drying, thereby effectively improving the mechanical properties of the film.

[0023] Preferably, as a further specific embodiment, the starch is one or more of corn starch, potato starch, tapioca starch, sweet potato starch, wheat starch, and pea starch.

[0024] Preferably, as a further specific embodiment, the starch is corn starch or wheat starch or a mixture of corn starch and wheat starch in a mass ratio of (3:1) to (1:1); Preferably, corn starch and wheat starch are mixed in a mass ratio of 2:1.

[0025] In the selection of starch, starch with a higher proportion of branches is preferred. Branched starch is insoluble in water and is more conducive to the formation of crystal seeds. Corn starch or wheat starch itself has a larger proportion of branches, which is more conducive to crystallization, so it is preferred. The applicant has found through a lot of creative work that when corn starch and wheat starch are mixed, especially when they are mixed in a mass ratio of (3:1)-(1:1), the mechanical properties of the film itself will be better improved, and the film can achieve an ideal shading effect. More preferably, when corn starch and wheat starch are mixed in a mass ratio of 2:1, the proportion of branches can be effectively increased, thereby improving the performance of the film itself.

[0026] Preferably, as a further specific embodiment, the water-soluble sugar or water-soluble sugar alcohol is a water-soluble sugar alcohol; Preferably, the water-soluble sugar alcohol is one or more of mannitol, xylitol, maltitol, lactitol or erythritol; Preferably, the water-soluble sugar alcohol is maltitol or a mixture of maltitol and xylitol in a mass ratio of (5:1) to (1:1); Preferably, the water-soluble sugar alcohol is a mixture of maltitol and xylitol in a mass ratio of 3:1.

[0027] The water-soluble sugar alcohols are maltitol and xylitol in a mass ratio of 5:1, 4:1, 2:1 or 1:1.

[0028] In the present invention, the performance of water-soluble sugar alcohols is better than that of water-soluble sugars; compared with water-soluble sugar alcohols, sugar alcohols themselves have better stability and can make crystals more delicate. Among sugar alcohols, the present invention prefers maltitol. Compared with other sugar alcohols, maltitol has a lower hydroxyl content, weaker interaction with water molecules, and is more likely to precipitate crystals. And it has a cyclic branched structure, the molecules are more likely to stack and interweave, and the crystals formed are more stable than those with other straight-chain sugar alcohols. Through a lot of creative work, the present invention found that maltitol and xylitol are mixed in a mass ratio of (5:1)-(1:1), preferably in a mass ratio of 3:1, which can form a more stable microstructure between molecules, thereby making the crystallization effect better and further improving the whiteness of the prepared film.

[0029] The present invention also provides a method for preparing an opaque film agent that replaces titanium dioxide, comprising: Add active ingredients, polymer film-forming materials, water-soluble sugars or sugar alcohols, starch, surfactants and water in sequence, stir evenly to obtain slurry; The slurry is degassed, coated, and dried to obtain the product.

[0030] Preferably, as a further specific implementation, the programmed drying is divided into two stages, the first stage is drying at a temperature of 40°C-60°C; the second stage is drying at a temperature of 100°C-140°C.

[0031] Preferably, as a further specific implementation, the drying time of the first stage is 2 min-5 min; the drying time of the second stage is 5 min-10 min.

[0032] In the present invention, the drying temperature and drying time of the two stages are extremely important for the present invention. The first stage of the programmed temperature is dried at 40℃-60℃ for 2min-5min. If the drying temperature is too high or the drying time is too long, the moisture on the surface of the film will evaporate too quickly, which will make the film surface easy to form a skin; if the drying temperature is too low or the drying time is too short, the purpose of preheating cannot be achieved, and the film is prone to form a skin or surface cracks during high-temperature drying in the second stage. The second stage of the programmed temperature is dried at 100℃-140℃ for 5min-10min. If the drying temperature is too high or the drying time is too long, the film will be over-dried and lose water and easily break; if the drying temperature is too low or the drying time is too short, crystals on the film surface are not easy to precipitate, and it is difficult to form a white opaque effect.

[0033] Compared with the prior art, the present invention has the following beneficial effects: (1) The film prepared by the present invention utilizes a combination of starch and water-soluble sugars or sugar alcohols to make the film present a white and opaque appearance, thereby providing a feasible solution technology for replacing titanium dioxide in the film formulation and improving safety.

[0034] (2) The film-forming composition of the present invention can be made into a film whose white color is stable for a long time without falling off from the surface, and the film-forming composition has excellent solubility. DETAILED DESCRIPTION

[0035] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] Example 1 Polymer film-forming material: maltodextrin 20g Water-soluble sugars or water-soluble sugar alcohols: sucrose 40g Starch: sweet potato starch 1g Surfactant: Sucrose fatty acid ester 2g Active ingredient: Rupatadine 7g Other ingredients 30g Add 7g of active ingredient rupatadine, 20g of polymer film-forming material maltodextrin, 40g of water-soluble sugar or water-soluble sugar alcohol sucrose, 1g of sweet potato starch (the starch particle size used in this embodiment is 1 μm), 2g of surfactant sucrose fatty acid ester, 30g of other auxiliary materials and water in sequence, stir evenly to obtain slurry; degas the slurry and then apply it, and dry it by program. The drying temperature of the first stage is 40°C, the drying time is 2min, and the drying temperature of the second stage is 100°C, and the drying time is 5min.

[0037] Example 2 Polymer film-forming material: polyvinyl alcohol 23g Water-soluble sugars or water-soluble sugar alcohols: mannitol 20g Starch: potato starch 5g Surfactant: Tween 2g Active ingredient: Lentinan 50g Add 50g of active ingredient Lentinan, 23g of polymer film-forming material polyvinyl alcohol, 20g of water-soluble sugar or sugar alcohol mannitol, 5g of potato starch (the starch particle size used in this embodiment is 50μm), 2g of surfactant Tween and water in sequence, stir evenly to obtain slurry; degas the slurry and apply it, and dry it in a program. The drying temperature of the first stage is 60°C and the drying time is 5min, and the drying temperature of the second stage is 140°C and the drying time is 10min.

[0038] Example 3 Polymer film-forming material: Hydroxypropyl cellulose 80g Water-soluble sugar or water-soluble sugar alcohol: xylitol 10g Starch: 3g tapioca starch Surfactant: Poloxamer 0.5g Other excipients: 6.5g Add 80g of polymer film-forming material hydroxypropyl cellulose, 10g of water-soluble sugar or water-soluble sugar alcohol xylitol, 3g of starch cassava starch (the starch particle size used in this embodiment is 2μm), 0.5g of surfactant poloxamer, 6.5g of other auxiliary materials and water in sequence, stir evenly to obtain slurry; degas the slurry and then apply it, and dry it in a program. The drying temperature of the first stage is 42°C and the drying time is 3min, and the drying temperature of the second stage is 120°C and the drying time is 8min.

[0039] Example 4 Polymer film-forming material: Hydroxyethyl cellulose 50g Water-soluble sugars or water-soluble sugar alcohols: 32g maltose Starch: pea starch 4g Surfactant: Polyoxyethylene oleyl alcohol ether 2g Active ingredient: Propolis 12g Add 12g of active ingredient propolis, 50g of polymer film-forming material hydroxyethyl cellulose, 32g of water-soluble sugar or water-soluble sugar alcohol maltose, 4g of pea starch (the starch particle size used in this embodiment is 20μm), 2g of surfactant polyoxyethylene oleyl alcohol ether and water in sequence, stir evenly to obtain slurry; degas the slurry and then apply it, and program dry it to obtain the slurry. The drying temperature of the first stage is 50°C, the drying time is 3min, and the drying temperature of the second stage is 115°C, and the drying time is 7min.

[0040] Example 5 Polymer film-forming material: Hydroxypropyl methylcellulose 60g Water-soluble sugars or water-soluble sugar alcohols: lactitol 15g Starch: Wheat starch 4g Surfactant: Glyceryl stearate 1g Active ingredients: Probiotics 15g Other auxiliary materials 5g Add 15g of active ingredient probiotics, 60g of polymer film-forming material hydroxypropyl methylcellulose, 15g of water-soluble sugar or sugar alcohol lactitol, 4g of starch wheat starch (the starch particle size used in this embodiment is 15μm), 1g of surfactant stearyl glyceride, 5g of other auxiliary materials and water in sequence, stir evenly to obtain slurry; degas the slurry and then apply it, and program dry it to obtain. The drying temperature of the first stage is 55°C and the drying time is 4min, and the drying temperature of the second stage is 130°C and the drying time is 6min.

[0041] Example 6 The specific preparation steps of the composition are the same as those of Example 5, except that the mass ratio of lactitol to stearin is changed to 12:1, and the total grams of the two remain unchanged, including 14.8 g of lactitol and 1.2 g of stearin.

[0042] Example 7 The specific preparation steps of the composition are the same as those of Example 5, except that the mass ratio of lactitol to stearin is changed to 17:1, and the total grams of the two remain unchanged, including 15.1 g of lactitol and 0.9 g of stearin.

[0043] Example 8 The specific preparation steps of the composition are the same as those of Example 5, except that the mass ratio of lactitol to stearin is changed to 19:1, and the total grams of the two remain unchanged, including 15.2 g of lactitol and 0.8 g of stearin.

[0044] Example 9 The specific preparation steps of the composition are the same as those of Example 8, except that the starch is replaced by corn starch, and the weight of the starch itself remains unchanged.

[0045] Example 10 The specific preparation steps of the composition are the same as those of Example 8, except that the starch is replaced by corn starch and wheat starch, and the mass ratio of corn starch to wheat starch is 3:1, and the grams of starch itself remains unchanged, including 3g of corn starch and 1g of wheat starch.

[0046] Embodiment 11 The specific preparation steps of the composition are the same as those of Example 8, except that the starch is replaced by corn starch and wheat starch, and the mass ratio of corn starch to wheat starch is 2:1, and the grams of starch itself remains unchanged, including 2.7g corn starch and 1.3g wheat starch.

[0047] Example 12 The specific preparation steps of the composition are the same as those of Example 8, except that the starch is replaced by corn starch and wheat starch, and the mass ratio of corn starch to wheat starch is 1:1, and the grams of starch itself remains unchanged, including 2g of corn starch and 2g of wheat starch.

[0048] Embodiment 13 The specific preparation steps of the composition are the same as those of Example 11, except that the water-soluble sugar or water-soluble sugar alcohol is replaced by fructose, and the grams of the water-soluble sugar or water-soluble sugar alcohol itself remains unchanged.

[0049] Embodiment 14 The specific preparation steps of the composition are the same as those of Example 11, except that the water-soluble sugar or water-soluble sugar alcohol is replaced by maltitol, and the grams of the water-soluble sugar or water-soluble sugar alcohol itself remains unchanged.

[0050] Embodiment 15 The specific preparation steps of the composition are the same as those of Example 11, except that the water-soluble sugars or water-soluble sugar alcohols are replaced by maltitol and xylitol, and the mass ratio of maltitol to xylitol is 5:1, and the grams of the water-soluble sugars or water-soluble sugar alcohols themselves remain unchanged, including 12.5g of maltitol and 2.5g of xylitol.

[0051] Example 16 The specific preparation steps of the composition are the same as those of Example 11, except that the water-soluble sugars or water-soluble sugar alcohols are replaced by maltitol and xylitol, and the mass ratio of maltitol to xylitol is 3:1, and the grams of the water-soluble sugars or water-soluble sugar alcohols themselves remain unchanged, including 11.2g of maltitol and 3.8g of xylitol.

[0052] Embodiment 17 The specific preparation steps of the composition are the same as those of Example 11, except that the water-soluble sugars or water-soluble sugar alcohols are replaced by maltitol and xylitol, and the mass ratio of maltitol to xylitol is 1:1, and the grams of the water-soluble sugars or water-soluble sugar alcohols themselves remain unchanged, including 7.5g of maltitol and 7.5g of xylitol.

[0053] Embodiment 18 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio of maltitol to xylitol to stearin is changed to 8:1, and the total grams of the two remain unchanged, including 14.3g of maltitol and xylitol and 1.7g of stearin.

[0054] Embodiment 19 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio of maltitol to xylitol to stearin is changed to 25:1, and the total grams of the two remain unchanged, including 15.4g of maltitol and xylitol and 0.6g of stearin.

[0055] Embodiment 20 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio between corn starch and wheat starch is changed to 6:1, and the total grams of the two remain unchanged, including 3.4g of corn starch and 0.6g of wheat starch.

[0056] Embodiment 21 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio between corn starch and wheat starch is changed to 1:3, and the total grams of the two remain unchanged, wherein corn starch is 1g and wheat starch is 3g.

[0057] Embodiment 22 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio of maltitol to xylitol is changed to 1:4, and the total grams of the two remain unchanged, wherein maltitol is 3g and xylitol is 12g.

[0058] Embodiment 23 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio of maltitol to xylitol is changed to 7:1, and the total grams of the two remain unchanged, with 13.1 g of maltitol and 1.9 g of xylitol.

[0059] Embodiment 24 The specific preparation steps of the composition are the same as those of Example 16, except that the drying temperature in the first stage is changed to 20°C.

[0060] Embodiment 25 The specific preparation steps of the composition are the same as those of Example 16, except that the drying temperature in the first stage is changed to 80°C.

[0061] Embodiment 26 The specific preparation steps of the composition are the same as those of Example 16, except that the drying temperature in the second stage is changed to 60°C.

[0062] Embodiment 27 The specific preparation steps of the composition are the same as those of Example 16, except that the drying temperature in the second stage is changed to 180°C.

[0063] Embodiment 28 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio between the water-soluble sugar or water-soluble sugar alcohol and the surfactant is changed to 0.5:1, and the total grams of the two remain unchanged, including 5.3g of maltitol and xylitol, and 10.7g of stearic acid glyceryl.

[0064] Embodiment 29 The specific preparation steps of the composition are the same as those of Example 16, except that the mass ratio between the water-soluble sugar or water-soluble sugar alcohol and the surfactant is changed to 44:1, and the total grams of the two remain unchanged, including 15.6g of maltitol and xylitol, and 0.4g of stearic acid glyceryl.

[0065] Comparative Example 1 The specific preparation steps of the composition are the same as those of Example 16, except that no water-soluble sugar or water-soluble sugar alcohol is used.

[0066] Comparative Example 2 The specific preparation steps of the composition are the same as those of Example 16, except that starch is not used.

[0067] Comparative Example 3 The specific preparation steps of the composition are the same as those of Example 16, except that no surfactant is used.

[0068] Comparative Example 4 The specific preparation steps of the composition are the same as those of Example 16, except that the starch particle size used is 0.5 μm.

[0069] Comparative Example 5 The specific preparation steps of the composition are the same as those of Example 16, except that the starch particle size used is 60 μm.

[0070] Experimental example The film preparations obtained in the examples and comparative examples were tested, and the test data are shown in the following Table 1. The dissolution time was measured according to the Chinese Pharmacopoeia Disintegration Time Test Method (General Rule 0921).

[0071] Table 1 Appearance and properties of membranes

[0072] Based on the above data, we can draw the following conclusions: The film prepared according to the scheme of Example 16 has the best performance, so the scheme of Example 16 is the best scheme of the present invention.

[0073] It can be seen from the experimental data that adding starch and water-soluble sugars or water-soluble sugar alcohols to the film-forming material causes crystals to gradually precipitate on the surface of the film during the drying process, so that the prepared film can also present an opaque white color without adding titanium dioxide, and can replace the titanium dioxide in the orally dissolving film to present a white color, thereby improving safety. In addition, the film of the present invention can maintain a stable white color for a long time without falling off from the surface, and has excellent dissolution performance.

[0074] By comparing the experimental results of Example 14 and Example 11, it can be seen that when the preferred water-soluble sugar or water-soluble sugar alcohol is maltitol, the light-shielding performance of the obtained film is better. Because maltitol has a lower hydroxyl content than other sugar alcohols, it has a weaker interaction with water molecules and is more likely to precipitate crystals. In addition, it has a cyclic branched structure, and the molecules are more likely to stack and interweave, and the crystals formed are more stable than those formed by other straight-chain sugar alcohols.

[0075] In the experimental process of Example 13 and Example 14, the soluble sugar alcohol or sugar component was replaced, and the transmittance and dissolution time of the film prepared after the replacement were slightly lower than those of Example 16. It can be seen that compared with Examples 13-14, the film prepared in Example 16 has a higher appearance opacity, which can confirm that water-soluble sugar alcohols have better performance than water-soluble sugars, and water-soluble sugar alcohols can make crystals more delicate. At the same time, by comparing Examples 13-14 with Example 16, it can be seen that the effect of mixing maltitol and xylitol is greater than the effect of using maltitol alone, and the effect of using fructose alone. On this basis, the present invention has also discovered through a lot of creative work that maltitol and xylitol are better when mixed in a certain mass ratio. By comparing Example 16 with Examples 15-17 and Examples 22-23, it can be seen that when maltitol and xylitol are mixed in a mass ratio of (5:1)-(1:1), and the preferred mass ratio is 3:1, a more stable microstructure can be formed between the molecules, thereby achieving a better crystallization effect and further improving the whiteness of the film.

[0076] Examples 9-12 changed the type of starch and the ratio between starches. From the experimental results, it can be seen that compared with Example 9, the film prepared in Example 11 has a higher appearance opacity, which shows that the effect of using corn starch and wheat starch in combination is greater than using corn starch alone; at the same time, by comparing Example 11 with Examples 10 and 12, it can be seen that when the mass ratio of corn starch to wheat starch is 2:1, the light-shielding performance of the prepared film is improved. By comparing Example 16 with Examples 20-21, Examples 20-21 changed the ratio between corn starch and wheat starch on the basis of Example 16. The experimental results show that when the content of a certain component is too high or too low, the light-shielding performance of the film will be reduced, thereby making it impossible to achieve the purpose of the present invention. The reason is that when the two are proportionally changed within the range selected by the present invention, the proportion of starch branches can be effectively increased, thereby further improving the light-shielding property of the film and improving the physical properties of the film.

[0077] Embodiment 6-8, embodiment 18-19, embodiment 28-29 and comparative example 3 adjust the ratio of water-soluble sugar or water-soluble sugar alcohol to surfactant or one of the components. By comparing embodiment 16 and comparative example 3, it can be seen that when no surfactant is used, the surface tension in starch cannot be reduced, which ultimately leads to poor film quality or inability to form a film. By comparing the experimental results of embodiment 6-8, it can be found that the light transmittance of the film prepared by embodiment 8 is lower than that of embodiment 6-7, which can confirm that the ratio of water-soluble sugar or water-soluble sugar alcohol to surfactant has an impact on the effect of the film finally prepared. The reason is that in the process of preparing the film, hydrogen bonds are formed between the hydrophilic group of the surfactant and the water-soluble film-forming material, reducing the surface tension, thereby reducing the viscosity of the slurry, making sugars or sugar alcohols easy to diffuse and crystallize. At the same time, the repulsion of the surfactant to water molecules is greater than the attraction, which will accelerate the evaporation of water. Thereby, crystals are formed quickly, providing whiteness for the film. By comparing Example 16, Example 18-19 and Example 28-29, it can be seen that the mass ratio of water-soluble sugars or water-soluble sugar alcohols to surfactants will also ultimately affect the morphology of film formation by affecting the microcrystals. The ratio between water-soluble sugars or water-soluble sugar alcohols and surfactants is usually between (1:1)-(40:1), and the preferred mass ratio is (10:1)-(20:1); when the surfactant ratio is too low, the slurry viscosity is too large, the crystallization is uneven, and the speed is slow. When the film is just dried, it still cannot be completely crystallized. If it is over-dried, it is easy to break, affecting the mechanical properties of the film; when the surfactant ratio is too high, the surface interface energy of the crystalline material is reduced, the formation of crystal seeds is inhibited, and it is difficult to crystallize. And it can be seen from Example 16 that it is more preferred that the mass ratio of water-soluble sugars or water-soluble sugar alcohols to surfactants is 19:1, which can ensure that the water-soluble sugars or water-soluble sugar alcohols are completely crystallized and can be dried quickly, thereby effectively improving the mechanical properties of the film.

[0078] Example 16 and Comparative Example 2 compare the particle size of starch with the use of starch. In the process of preparing the film, starch and water-soluble sugars or water-soluble sugar alcohols precipitate crystals together when the film is dried, which increases the opacity of the film. In the selection of starch, starch with a higher proportion of branches is preferred. Branched starch is insoluble in water and is more conducive to the formation of crystal seeds. Corn starch or wheat starch itself has a large proportion of branches, which is more conducive to crystallization. The applicant has found through a lot of creative work that the mixed use of corn starch and wheat starch can achieve a better shading effect. By comparing Example 16 and Comparative Examples 4-5, it can be seen that the particle size of starch will affect the crystallization effect of starch. When the particle size of starch is too large, the film-forming surface is rough and the white crystals are uneven; when the starch particle size is too small, it is not conducive to the formation of crystal seeds, which will affect the whiteness of the subsequent film. Therefore, the particle size of starch is usually between 1 μm and 50 μm, preferably between 2 μm and 20 μm, and more preferably 15 μm particle size starch can better interact with other auxiliary materials, so that the prepared film has a white and opaque appearance, and the appearance of the film can be made better.

[0079] By comparing the preparation methods of Example 16 and Examples 24-27, it can be seen that the drying temperature during staged drying will affect the mechanical properties of the film. It can be seen from the data of Example 16 that when the drying temperature is in an appropriate range, the performance of the film formed is significantly better than that of Examples 24-27. Because the drying temperature in the first stage is too high, the water on the surface of the film evaporates too quickly, which makes the surface of the film easy to form a crust and crack, while the drying temperature is too low, and crystals on the surface of the film are not easy to precipitate, and it is difficult to form a white opaque effect. Therefore, only when the drying temperature in the first stage is within the range of 40°C-60°C and the drying temperature in the second stage is within the range of 100°C-140°C can a film with sufficient whiteness be prepared.

[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An opaque film agent for replacing titanium dioxide, characterized in that: In terms of mass percentage, it is mainly made from the following raw materials: Polymer film-forming materials 20%-80%; Water-soluble sugars or water-soluble sugar alcohols 10%-40%; Starch 1%-5%; Surfactant 0.5%-2%; Active ingredient 0%-50%; Wherein, the particle size of the starch is 1 μm-50 μm.

2. The opaque film agent for replacing titanium dioxide according to claim 1, characterized in that: The particle size of the starch is 2 μm-20 μm; Preferably, the starch has a particle size of 15 μm.

3. The opaque film agent for replacing titanium dioxide according to claim 1, characterized in that: The mass ratio of the water-soluble sugar or water-soluble sugar alcohol to the surfactant is (10:1)-(20:1); Preferably, the mass ratio of the water-soluble sugar or water-soluble sugar alcohol to the surfactant is 19:

1.

4. The opaque film agent for replacing titanium dioxide according to claim 1, characterized in that: The starch is one or more of corn starch, potato starch, cassava starch, sweet potato starch, wheat starch and pea starch.

5. The opaque film agent for replacing titanium dioxide according to claim 4, characterized in that: The starch is corn starch or wheat starch or a mixture of corn starch and wheat starch in a mass ratio of (3:1) to (1:1); Preferably, corn starch and wheat starch are mixed in a mass ratio of 2:

1.

6. The opaque film agent for replacing titanium dioxide according to claim 1, characterized in that: The water-soluble sugar or water-soluble sugar alcohol is a water-soluble sugar alcohol; Preferably, the water-soluble sugar alcohol is one or more of mannitol, xylitol, maltitol, lactitol or erythritol; Preferably, the water-soluble sugar alcohol is maltitol or a mixture of maltitol and xylitol in a mass ratio of (5:1) to (1:1); Preferably, the water-soluble sugar alcohol is a mixture of maltitol and xylitol in a mass ratio of 3:

1.

7. A method for preparing an opaque film agent for replacing titanium dioxide as claimed in any one of claims 1 to 6, characterized in that: The steps include: Add active ingredients, polymer film-forming materials, water-soluble sugars or sugar alcohols, starch, surfactants and water in sequence, stir evenly to obtain slurry; The slurry is degassed, coated, and dried to obtain the product.

8. The method for preparing an opaque film agent replacing titanium dioxide according to claim 7, characterized in that: The programmed drying is divided into two stages, the first stage is drying at a temperature of 40°C-60°C; the second stage is drying at a temperature of 100°C-140°C.

9. The method for preparing an opaque film agent replacing titanium dioxide according to claim 8, characterized in that: The drying time of the first stage is 2 min-5 min; the drying time of the second stage is 5 min-10 min.