PVG conveying belt cover rubber composition, cover rubber, preparation method of cover rubber and PVG conveying belt
By using nitrile rubber, neoprene and triphenyl phosphate and other materials in the PVG conveyor belt, a covering glue that can be quickly worn out under high temperature conditions is designed, which solves the problem of excessive friction temperature of traditional conveyor belt rollers. Meets the demand for physical strength and flame retardant performance of modern mines.
Patent Information
- Application Number
- CN202411353844.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-26
AI Technical Summary
Under high-strength and thick-cover glue, the roller friction temperature is easily exceeded, and cannot be worn out quickly, which cannot meet the requirements of modern large mines for physical strength and flame retardant performance.
Nitrile rubber and neoprene are used as the main material, combined with triphenyl phosphate, white carbon black and other materials, a low-melting point flame retardant plasticization system and reinforcement filling system are designed, and the combination of vulcanizing agent and anti-aging agent is used to form a high A cover glue composition that is strong and capable of rapid breaking.
It realizes high strength and rapid wear of PVG conveyor belt covering glue, meets the roller friction temperature requirements of the coal industry standard MT/T914-2019, and extends the service life of the conveyor belt.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber conveyor belts, in particular to a PVG conveyor belt covering rubber composition, a covering rubber and a preparation method thereof, and a PVG conveyor belt. Background Art
[0002] PVG conveyor belts are mainly used in underground coal mines, where flame retardant properties are highly required. They are mainly composed of two parts: covering rubber and skeleton material. The skeleton material is generally woven from polyester warp and nylon weft to provide strength support for material transportation, but these two materials are flammable and need to be impregnated with PVC paste resin and a large amount of flame retardant to improve the flame retardant properties. In order to improve the wear resistance of the conveyor belt surface and extend its service life, a layer of rubber covering rubber is bonded and vulcanized on the surface of the skeleton material. Considering the compatibility with PVC resin, nitrile rubber is generally used as the main rubber of the covering rubber, but nitrile rubber is also flammable and needs to be filled with a large amount of flame retardant to improve the flame retardant properties of the covering rubber.
[0003] The roller friction test is the basic safety performance required by the coal industry standard MT / T914-2019 for PVG conveyor belts. The test sample cover rubber and the roller surface gradually heat up under the action of friction. At this time, due to the presence of a large amount of flame retardants, the cover rubber will quickly dehydrate into carbon at high temperature, forming a stable, strong and lubricated carbon layer. The roller slips on the conveyor belt surface and cannot wear off the belt body. The conveyor belt is a poor conductor of heat. When the heat generated by friction is greater than the heat dissipation of the system, the roller friction temperature will slowly increase. Under long-term continuous friction conditions, the roller friction temperature can easily exceed the standard requirement of 325°C, especially when the cover rubber thickness is greater than 3mm.
[0004] With the development of modern large-scale mines, the requirements for the physical strength of conveyor belts are getting higher and higher, and the thickness of the matching covering rubber is also getting thicker and thicker. The covering rubber with traditional formula can no longer effectively meet the requirements of customers and standards, and cannot be quickly worn off, making the friction temperature of the conveyor belt roller easily exceed the standard. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a PVG conveyor belt covering rubber composition, a covering rubber and a preparation method thereof, and a PVG conveyor belt. The covering rubber provided by the present invention not only has high strength, but also can be quickly worn off, thereby solving the industry problem that the friction temperature of the roller of a high-strength and thick-covered PVG conveyor belt is prone to exceed the standard.
[0006] The present invention provides a PVG conveyor belt covering rubber composition, comprising:
[0007] 50~80 parts of nitrile rubber;
[0008] 5~30 parts of chloroprene rubber;
[0009] PVC resin 10~40 parts;
[0010] 10-30 parts of triphenyl phosphate;
[0011] 20-40 parts of tri(2-chloroethyl) phosphate;
[0012] 5-15 parts of antimony trioxide;
[0013] Carbon black 20~40 parts;
[0014] 5-20 parts of white carbon black;
[0015] 2.3~5 parts of vulcanizing agent;
[0016] 1.5~7 parts of activator;
[0017] 2~6 parts of antioxidant.
[0018] In certain embodiments of the present invention, the vulcanizing agent is selected from at least one of sulfur, 4,4′-dimorpholine disulfide, N-tert-butyl-2-benzothiazole sulfenamide, N-cyclohexyl-2-benzothiazole sulfenamide, and tetramethylthiuram disulfide; the activator is selected from at least one of zinc oxide, stearic acid, and magnesium oxide; and the antioxidant is selected from at least one of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 9,9-dimethylacridine, and microcrystalline paraffin.
[0019] The PVG conveyor belt covering rubber composition provided by the present invention improves the flame retardant performance of the main rubber material and reduces the addition amount of the flame retardant by designing nitrile rubber and chloroprene rubber as the covering rubber main rubber material; designs the flame retardant triphenyl phosphate as a solid flame retardant plasticizer, utilizes the low melting point property of triphenyl phosphate to soften the covering rubber under high temperature friction conditions, delays the carbonization speed of the covering rubber, and avoids the formation of a stable, strong and lubricated carbon layer; designs white carbon black as a filler, utilizes the rigidity characteristic of white carbon black, grinds other materials with white carbon black as the core, accelerates the wear speed of the softened covering rubber, and enables the covering rubber to be quickly worn off; the PVG conveyor belt covering rubber obtained by the composition has high strength and can be quickly worn off, thereby solving the industry problem that the friction temperature of the roller of the high-strength and thick covering rubber PVG conveyor belt is easily exceeded.
[0020] Preferably, the PVG conveyor belt covering rubber composition provided by the present invention further comprises:
[0021] Auxiliary reinforcing agent 5~10 parts;
[0022] Auxiliary flame retardant plasticizer 10~30 parts;
[0023] 10~30 parts of flame retardant synergist.
[0024] In certain embodiments of the present invention, the auxiliary reinforcing agent is selected from at least one of calcium carbonate, calcined clay, and aluminum silicate; the auxiliary flame retardant plasticizer is selected from at least one of triaryl phosphate, 52# chlorinated paraffin, and triethyl phosphate; and the flame retardant synergist is selected from at least one of aluminum hydroxide, zinc borate, and melamine cyanurate.
[0025] The PVG conveyor belt covering rubber composition provided by the present invention adopts a blend of nitrile rubber and chloroprene rubber as the main rubber material. The nitrile rubber has good compatibility with the PVC paste resin impregnated in the skeleton material, which can effectively ensure the bonding strength between the covering rubber and the skeleton material. The 3305 type is adopted, and the process performance is good. The chloroprene rubber has a higher oxygen index, which improves the flame retardancy of the main rubber material, and the SN121 type is adopted. At the same time, the PVC paste resin is used, which has flame retardancy and improves compatibility with the skeleton material. At the same time, it begins to melt at more than 160°C, which slows down the carbonization rate of the covering rubber. The PVC resin model adopts CPM-31. In some embodiments of the present invention, the nitrile rubber is 3305 brand nitrile rubber, the PVC resin is LF-51L brand PVC resin, and the chloroprene rubber is SN121 brand chloroprene rubber.
[0026] The PVG conveyor belt covering rubber composition provided by the present invention adopts flame retardant triphenyl phosphate and tri(2-chloroethyl) phosphate as softening plasticizing system; wherein triphenyl phosphate is used as solid flame retardant plasticizer, which has a low melting point of 47°C to 53°C, and can absorb heat and melt in the early stage of friction heat generation, so that the covering rubber softens under high temperature friction conditions, promotes rapid wear of the covering rubber, and avoids the formation of a strong, lubricating, and wear-resistant surface carbon layer; and its phosphorus content is about 9.5%, and it has good flame retardant properties. And tri(2-chloroethyl) phosphate is used as a liquid flame retardant plasticizer, and its phosphorus content is about 10.8%, and its chlorine content is 37.3%, which is a high-efficiency flame retardant with plasticizing effect. In certain embodiments of the present invention, the PVG conveyor belt covering rubber composition also includes an auxiliary flame retardant plasticizer, and the auxiliary flame retardant plasticizer of the present invention can play a role in avoiding the precipitation of plasticizers, and the auxiliary flame retardant plasticizer is preferably selected from triaryl phosphate, which is used as an auxiliary flame retardant plasticizer and has flame retardant effect.
[0027] The PVG conveyor belt covering rubber composition provided by the present invention adopts antimony trioxide as a flame retardant, which can be used together with tris(2-chloroethyl) phosphate in the softening and plasticizing system of the present invention as the flame retardant system of the covering rubber formula of the present invention. The flame retardant system effectively reduces the flaming combustion time after the alcohol blowtorch is removed by using a chlorine system and an antimony system. The flame retardant system of the present invention also includes a flame retardant synergist, and aluminum hydroxide is preferably used as a flame retardant synergist. When aluminum hydroxide is thermally decomposed, it releases crystal water. This process is a strong endothermic reaction, absorbing a large amount of heat, which can play a role in cooling the polymer. At the same time, the water vapor generated by the reaction can dilute the combustible gas and inhibit the spread of combustion.
[0028] The PVG conveyor belt covering rubber composition provided by the present invention uses carbon black and white carbon black as a reinforcing filling system; the reinforcing filling system of the present invention avoids the use of carbon-forming and strong acidic materials, uses carbon black as a reinforcing filling system, and reduces the amount of carbon black used as much as possible on the basis of ensuring physical strength. White carbon black is used as an auxiliary filler, and the rigid characteristics of white carbon black are utilized to grind other materials with white carbon black as the core, thereby accelerating the wear rate of the softened covering rubber and enabling the covering rubber to be quickly ground off. The composition of the present invention also includes an auxiliary reinforcing agent, and the auxiliary reinforcing agent is preferably selected from calcium carbonate. By using 325 mesh calcium carbonate at the same time, the calcium carbonate with a larger diameter has a grinding effect, which can promote the wear of the covering rubber, and at the same time, calcium carbonate can improve the thermal stability of the PVC resin. In some embodiments of the present invention, the carbon black is N234 carbon black, N115 carbon black or N220 carbon black.
[0029] The PVG conveyor belt covering rubber composition provided by the present invention adopts a vulcanizing agent to construct a vulcanization system, preferably an effective vulcanization system using a low amount of sulfur and a sulfur donor 4,4'-dithiodimorpholine. When 4,4'-dithiodimorpholine is used as a vulcanizing agent, active sulfur can be decomposed at the vulcanization temperature without scorching, which is beneficial to the discharge of air trapped between the covering rubber and the belt blank during the molding process.
[0030] The PVG conveyor belt covering rubber composition provided by the present invention includes an activator, preferably zinc oxide and stearic acid are used as the activator. They are combined to form zinc stearate salt, participate in the vulcanization reaction process, reduce the number of polysulfide bonds, and thus improve the heat resistance and aging resistance.
[0031] The PVG conveyor belt covering rubber composition provided by the present invention adopts an antioxidant to construct an anti-aging system, and preferably uses N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and microcrystalline wax in combination as the anti-aging system, wherein N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine has excellent resistance to thermal oxygen aging, ozone aging and flex cracking; and the microcrystalline wax can form a protective film on the surface of the covering rubber to isolate the erosion of oxygen and ozone in the air.
[0032] In some embodiments of the present invention, the PVG conveyor belt covering rubber composition of the present invention includes: 50-80 parts of nitrile rubber; 5-30 parts of chloroprene rubber; 10-40 parts of PVC resin; 10-30 parts of triphenyl phosphate; 20-40 parts of tri(2-chloroethyl) phosphate; 10-30 parts of triaryl phosphate; 5-15 parts of antimony trioxide; 20-40 parts of carbon black; 5-20 parts of white carbon black; 5-10 parts of calcium carbonate; 10-30 parts of aluminum hydroxide; 0.3-1 parts of sulfur; 2-4 parts of 4,4′-dithiodimorpholine; 1-5 parts of zinc oxide; 0.5-2 parts of stearic acid; 1-3 parts of N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine; and 1-3 parts of microcrystalline paraffin.
[0033] In some other embodiments of the present invention, the PVG conveyor belt covering rubber composition of the present invention includes: 50-55 parts of nitrile rubber; 10-15 parts of chloroprene rubber; 35-40 parts of PVC resin; 10-20 parts of triphenyl phosphate; 20-25 parts of tri(2-chloroethyl) phosphate; 10-15 parts of triaryl phosphate; 5-15 parts of antimony trioxide; 25-28 parts of carbon black; 8-12 parts of white carbon black; 5-10 parts of calcium carbonate; 10-15 parts of aluminum hydroxide; 0.3-1 part of sulfur; 2-4 parts of 4,4′-dithiodimorpholine; 1-5 parts of zinc oxide; 0.5-2 parts of stearic acid; 1-3 parts of N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine; and 1-3 parts of microcrystalline paraffin.
[0034] The present invention provides a PVG conveyor belt covering rubber, which is obtained from the composition described in any of the above technical solutions. The present invention also provides a method for preparing the above PVG conveyor belt covering rubber, comprising the following steps:
[0035] S1) mixing nitrile rubber, chloroprene rubber, PVC resin, triphenyl phosphate, antimony trioxide, activator and antioxidant for the first time, and then adding tri(2-chloroethyl) phosphate, auxiliary flame retardant plasticizer, carbon black and white carbon black for the first time to obtain a first stage of rubber;
[0036] S2) After the rubber obtained in step S1) is left to stand, a vulcanizing agent is added to perform a second mixing and a second rubber discharge, and after vulcanization, a PVG conveyor belt covering rubber is obtained.
[0037] The invention firstly mixes nitrile rubber, chloroprene rubber, PVC resin, triphenyl phosphate, antimony trioxide, an activator and an antioxidant for the first time, wherein the first mixing time is 60 s to 120 s, and then adds tris(2-chloroethyl) phosphate, an auxiliary flame retardant plasticizer, carbon black and white carbon black for the first debonding, wherein the temperature of the first debonding is 110° C. to 130° C., to obtain a rubber section;
[0038] After obtaining the first section of rubber, the first section of rubber is allowed to stand for a second time and then a vulcanizing agent is added for a second mixing and a second degumming; the standing time is 4 h to 24 h, preferably 8 h; the second degumming is started after the second mixing reaches 90° C. to 110° C. After the second mixing and the second degumming are performed, the obtained material is allowed to stand for 4 h to 24 h, preferably 8 h, and then vulcanized to obtain the PVG conveyor belt covering rubber.
[0039] The present invention also provides a PVG conveyor belt, which includes a substrate and a covering rubber covering the surface of the substrate, wherein the covering rubber is the above-mentioned PVG conveyor belt covering rubber or the PVG conveyor belt covering rubber obtained by the above-mentioned preparation method; specifically, the substrate is composed of warp, weft and paste, and the covering rubber covers the surface of the paste. In some embodiments of the present invention, the PVG conveyor belt is a trough surface PVG conveyor belt. In some embodiments of the present invention, the thickness of the covering rubber on the substrate surface of the PVG conveyor belt is 3 mm to 6 mm.
[0040] The present invention provides a PVG conveyor belt covering rubber composition, covering rubber and a preparation method thereof, and a PVG conveyor belt. The present invention adopts a low-melting-point solid flame-retardant plasticizer, which can absorb heat and melt in the early stage of frictional heat generation, so that the covering rubber softens under high-temperature friction conditions, avoids the formation of a strong, lubricated, and wear-resistant surface carbon layer, and is beneficial to the wear of the covering rubber under high-temperature conditions. By using an inorganic filler with strong rigidity, during the roller friction test process, other materials in the covering rubber are ground with the rigid filler as the core, thereby accelerating the wear rate of the softened covering rubber and allowing the covering rubber to be quickly worn off. Experiments show that the covering rubber provided by the present invention meets the MT / T914-2019 index requirements and solves the industry problem of the contradiction between flame retardancy and roller friction performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a schematic diagram of the product structure of the PVG conveyor belt of the present invention. DETAILED DESCRIPTION
[0042] The present invention discloses a PVG conveyor belt covering rubber composition, a covering rubber and a preparation method thereof, and a PVG conveyor belt. A person skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the above. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.
[0043] In the specific embodiment of the present invention, PVG conveyor belts with different formulas of covering rubber are prepared for testing, wherein the PVG conveyor belt is composed of weft, warp, paste and covering rubber, and the product structure is as follows: Figure 1 As shown, Figure 1 This is a schematic diagram of the product structure of the PVG conveyor belt of the present invention. Figure 1 Among them, 1 is the weft, 2 is the warp, 3 is the paste, and 4 is the covering glue.
[0044] The covering glue of the present invention is carried out according to the following steps:
[0045] 1) Ingredients: Nitrile rubber, chloroprene rubber, PVC resin, flame retardant plasticizer triphenyl phosphate, flame retardant antimony trioxide, flame retardant aluminum hydroxide, reinforcing agent calcium carbonate, zinc oxide, stearic acid, antioxidant N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and antioxidant microcrystalline wax are used as material package ①. Flame retardant plasticizer tri(2-chloroethyl) phosphate, flame retardant plasticizer triaryl phosphate, reinforcing agent carbon black, reinforcing agent white carbon black are used as material package ②. Sulfur and vulcanizing agent 4,4'-dithiodimorpholine are used as material package ③.
[0046] 2) Mixing of covering rubber: Set the speed of the internal mixer to 25 r / min, put material package ① into the internal mixer and mix for 60 s~120 s, then add material package ②, control the temperature at 110℃~130℃ to discharge the rubber, and make a first-stage rubber. After the first-stage rubber is left for 8 hours, put it into the internal mixer again and add material package ③, mix it to 90℃~110℃, control the temperature to discharge the rubber, and leave it for 8 hours before entering the vulcanization process.
[0047] The present invention will be further described below in conjunction with embodiments:
[0048] Example 1
[0049] The formula of the high flame retardant PVG conveyor belt covering rubber that can be quickly worn off in Example 1 of the present invention is composed of the components in parts by weight shown in Table 1:
[0050] Table 1
[0051]
[0052] Put material package ① into the internal mixer and mix for 90 seconds, then add material package ②, control the temperature at 130℃ to discharge the glue, and make a first-stage glue. After the first-stage glue is left for 8 hours, put it into the internal mixer again and add material package ③, mix it to 100℃, control the temperature to discharge the glue, and leave it for 8 hours before entering the vulcanization process.
[0053] The performance indicators of the conveyor belt covering rubber prepared in Example 1 are shown in Table 2 (conveyor belt grade 2500S, covering rubber thickness 4 mm+4 mm):
[0054] Table 2
[0055]
[0056] As can be seen from Table 2, the cover rubber of Example 1 of the present invention has excellent physical properties, is suitable for use on PVG conveyor belts with a cover rubber thickness of 3 mm to 4 mm, and has excellent wear resistance. At the same time, under high temperature conditions of roller friction, the cover rubber can be worn off within 15 minutes.
[0057] Example 2
[0058] The formula of the high flame retardant PVG conveyor belt covering rubber that can be quickly worn off in Example 2 of the present invention is composed of the components in parts by weight shown in Table 3:
[0059] Table 3
[0060]
[0061] Put material package ① into the internal mixer and mix for 90 seconds, then add material package ②, control the temperature at 125℃ to discharge the glue, and make a first-stage glue. After the first-stage glue is left for 8 hours, put it into the internal mixer again and add material package ③, mix it to 100℃ and control the temperature to discharge the glue, and then enter the vulcanization process after leaving it for 8 hours.
[0062] The performance indicators of the conveyor belt covering rubber prepared in Example 2 are shown in Table 4 (conveyor belt grade 2500S, covering rubber thickness 5 mm+5 mm):
[0063] Table 4
[0064]
[0065] The formula of Example 2 of the present invention has relatively balanced roller friction and physical properties, and is suitable for use in PVG conveyor belts with a cover rubber thickness of 4 mm to 5 mm along the trough surface, and can meet the needs of large modern mines with an annual coal throughput of 10 million tons. At the same time, under high temperature conditions of roller friction, the cover rubber can be worn off within 12 minutes.
[0066] Example 3
[0067] The formula of the high flame retardant PVG conveyor belt covering rubber that can be quickly worn off in Example 3 of the present invention is composed of the components in parts by weight shown in Table 5:
[0068] Table 5
[0069]
[0070] Put material package ① into the internal mixer and mix for 90 seconds, then add material package ②, control the temperature at 120℃ to discharge the glue, and make a first-stage glue. After the first-stage glue is left for 8 hours, put it into the internal mixer again and add material package ③, mix it to 95℃, control the temperature to discharge the glue, and leave it for 8 hours before entering the vulcanization process.
[0071] The performance indicators of the conveyor belt covering rubber prepared in Example 3 are shown in Table 6 (conveyor belt grade 2500S, covering rubber thickness 6 mm+6 mm):
[0072] Table 6
[0073]
[0074] The formula of Example 3 of the present invention has better roller friction performance. When the roller friction temperature reaches above 230°C, the covering rubber begins to delaminate from the skeleton material, accelerating the wear and tear of the sample. It is suitable for use in PVG conveyor belts with a covering rubber thickness of 5 mm to 6 mm along the trough surface, and can meet the needs of large modern mines with an annual coal throughput of 12 million tons.
[0075] Comparative Example 1
[0076] In order to compare the effects of two key materials, triphenyl phosphate and white carbon black, on the friction performance of the roller, based on Example 1, 10 parts of triaryl phosphate were used to replace 10 parts of triphenyl phosphate; and 8 parts of carbon black were used to replace 8 parts of white carbon black. The formula of Comparative Example 1 consists of the components in parts by weight shown in Table 7:
[0077] Table 7
[0078]
[0079] Put material package ① into the internal mixer and mix for 90 seconds, then add material package ②, control the temperature at 130℃ to discharge the glue, and make a first-stage glue. After the first-stage glue is left for 8 hours, put it into the internal mixer again and add material package ③, mix it to 100℃, control the temperature to discharge the glue, and leave it for 8 hours before entering the vulcanization process.
[0080] The performance indicators of the conveyor belt covering rubber prepared in Comparative Example 1 are shown in Table 8 (conveyor belt grade 2500S, covering rubber thickness 4 mm+4 mm):
[0081] Table 8
[0082]
[0083] It can be seen from Table 8 that without using triphenyl phosphate and white carbon black, the friction performance of the drum significantly exceeds the requirements of the MT / T914-2019 standard of the coal industry.
[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. PVG conveyor belt covering rubber composition, characterized in that: include: 50~80 parts of nitrile rubber; 5-30 parts of chloroprene rubber; 10~40 parts of PVC resin; 10-30 parts of triphenyl phosphate; 20-40 parts of tri(2-chloroethyl) phosphate; 5-15 parts of antimony trioxide; Carbon black 20~40 parts; 5-20 parts of white carbon black; 2.3~5 parts of vulcanizing agent; 1.5~7 parts of activator; 2~6 parts of antioxidant.
2. The PVG conveyor belt covering rubber composition according to claim 1, characterized in that: The vulcanizing agent is selected from at least one of sulfur, 4,4′-dimorpholine disulfide, N-tert-butyl-2-benzothiazole sulfenamide, N-cyclohexyl-2-benzothiazole sulfenamide and tetramethylthiuram disulfide; The activator is selected from at least one of zinc oxide, stearic acid and magnesium oxide; The antioxidant is selected from at least one of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 9,9-dimethylacridine and microcrystalline paraffin.
3. The PVG conveyor belt covering rubber composition according to claim 1, characterized in that: It also includes: Auxiliary reinforcing agent 5~10 parts; Auxiliary flame retardant plasticizer 10~30 parts; 10~30 parts of flame retardant synergist.
4. The PVG conveyor belt covering rubber composition according to claim 3, characterized in that: The auxiliary reinforcing agent is selected from at least one of calcium carbonate, calcined clay and aluminum silicate; The auxiliary flame retardant plasticizer is selected from at least one of triaryl phosphate, 52# chlorinated paraffin, and triethyl phosphate; The flame retardant synergist is selected from at least one of aluminum hydroxide, zinc borate and melamine cyanurate.
5. The PVG conveyor belt covering rubber composition according to claim 1, characterized in that: include: 50~80 parts of nitrile rubber; 5-30 parts of chloroprene rubber; 10~40 parts of PVC resin; 10-30 parts of triphenyl phosphate; 20-40 parts of tri(2-chloroethyl) phosphate; 10-30 parts of triaryl phosphate; 5-15 parts of antimony trioxide; Carbon black 20~40 parts; 5-20 parts of white carbon black; 5-10 parts of calcium carbonate; 10-30 parts of aluminum hydroxide; Sulfur 0.3~1 part; 2-4 parts of 4,4′-dithiodimorpholine; 1-5 parts of zinc oxide; 0.5~2 parts of stearic acid; 1-3 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine; 1~3 parts of microcrystalline paraffin.
6. The PVG conveyor belt covering rubber composition according to claim 5, characterized in that: include: 50-55 parts of nitrile rubber; Neoprene 10-15 parts; PVC resin 35~40 parts; 10-20 parts of triphenyl phosphate; 20-25 parts of tri(2-chloroethyl) phosphate; 10-15 parts of triaryl phosphate; 5-15 parts of antimony trioxide; Carbon black 25-28 parts; 8-12 parts of white carbon black; 5-10 parts of calcium carbonate; 10-15 parts of aluminum hydroxide; Sulfur 0.3~1 part; 2-4 parts of 4,4′-dithiodimorpholine; 1-5 parts of zinc oxide; 0.5~2 parts of stearic acid; 1-3 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine; 1~3 parts of microcrystalline paraffin. 7.PVG conveyor belt covering rubber, characterized by: Obtained from the composition described in any one of claims 1 to 6.
8. The method for preparing the PVG conveyor belt covering rubber according to claim 7, characterized in that: The following steps are involved: S1) mixing nitrile rubber, chloroprene rubber, PVC resin, triphenyl phosphate, antimony trioxide, activator and antioxidant for the first time, and then adding tri(2-chloroethyl) phosphate, auxiliary flame retardant plasticizer, carbon black and white carbon black for the first time to obtain a first stage of rubber; S2) After the rubber obtained in step S1) is left to stand, a vulcanizing agent is added to perform a second mixing and a second rubber discharge, and after vulcanization, a PVG conveyor belt covering rubber is obtained.
9. The preparation method according to claim 8, characterized in that: In step S1), the temperature of the first debinding is 110°C to 130°C; In step S2), the temperature of the second debinding is 90°C to 110°C. 10.PVG conveyor belt, characterized in that: It includes a substrate and a covering glue covering the surface of the substrate; The covering rubber is the PVG conveyor belt covering rubber as described in claim 7 or the PVG conveyor belt covering rubber obtained by any one of the preparation methods described in claims 8 to 9.
Citation Information
Cited By
Conveying belt for household garbage treatment and preparation method thereof
CN120737459A