Infrared thermal insulation film containing phosphino hydrotalcite and preparation method of infrared thermal insulation film
By using infrared insulation films containing phosphine-based hydrotalcite in agricultural films, the problem of poor infrared absorption performance of natural inorganic minerals is solved, significant infrared light absorption and excellent thermal insulation performance are achieved, and high requirements are suitable for modern agriculture. .
Patent Information
- Application Number
- CN202411285571.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The infrared absorption performance of natural inorganic mineral materials used in existing agricultural films is poor, which limits its insulation performance.
Using an infrared thermal insulation film containing phosphine-based hydrotalcite, zinc nitrate hexahydrate and aluminum nitrate nohydrate are uniformly dispersed, sodium hydroxide and sodium carbonate are added, and phosphine-based hydrotalcite is prepared through stirring, oven treatment, drying and other steps, and the Chlorinated polyethylene, functional filler, calcium and zinc stabilizer, diphenyl 2-ethylhexyl phosphate and antioxidant are mixed, and are refined and processed and pressurized to form an infrared insulation film.
It significantly improves the absorption effect and insulation performance of infrared light, ensures the quality and quality of the film, and is suitable for the high requirements of modern agriculture.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation film production, in particular to an infrared thermal insulation film containing phosphine-based hydrotalcite and a preparation method thereof. Background Art
[0002] With the high-demand development of modern agriculture, agricultural film has become one of the important means of production in agricultural production, and functional agricultural film has been sought after by different agricultural development needs. Most importantly, temperature is a major limiting factor in the development of agriculture, so the emergence of thermal insulation additives can improve the thermal insulation performance of agricultural film. At present, agricultural film is mainly doped with natural inorganic mineral materials with infrared absorption function such as kaolin, talc, wollastonite, sericite, calcium carbonate, etc., but the infrared absorption performance of the above natural inorganic minerals themselves is poor.
[0003] Based on this, the present invention provides an infrared thermal insulation film containing phosphine-based hydrotalcite and a preparation method thereof to solve the above-mentioned technical problems. Summary of the invention
[0004] The object of the present invention is to provide an infrared thermal insulation film containing phosphine-based hydrotalcite and a preparation method thereof. The prepared infrared thermal insulation film containing phosphine-based hydrotalcite not only has a significant absorption effect on infrared light, but also has excellent thermal insulation performance, effectively ensuring its quality.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] The first aspect of the present invention provides an infrared thermal insulation film containing phosphine-based hydrotalcite, which is composed of the following raw materials in parts by weight: 20 to 30 parts of chlorinated polyethylene, 10 to 14 parts of phosphine-based hydrotalcite, 3 to 6 parts of functional filler, 3 to 6 parts of calcium zinc stabilizer, 2 to 3 parts of diphenyl 2-ethylhexyl phosphate and 2 to 5 parts of antioxidant.
[0007] The present invention is further configured as follows: the preparation process of the phosphine-based hydrotalcite is as follows:
[0008] Evenly dispersing zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a first pre-formulated solution;
[0009] Evenly dispersing sodium hydroxide and sodium carbonate in deionized water to obtain a second solution;
[0010] The first pre-prepared liquid and the second pre-prepared liquid are added to water at 80-90° C. and 1250-1500 r / min in a volume ratio of 1:2-4, wherein the volume of the water is 2-3 times the sum of the volumes of the first pre-prepared liquid and the second pre-prepared liquid, and the mixture is kept warm and stirred for 60-80 minutes, and then placed in an oven at a constant temperature of 88-92° C. for 12-14 hours, filtered, washed with deionized water for 2-4 times, and then dried at 45-50° C. for 15-17 hours to obtain a base material;
[0011] The base material is dispersed in deionized water at a solid-liquid ratio of 0.22-0.28 g / mL to obtain a mixed solution, the mixed solution is mixed with a sodium dihydrogen phosphate aqueous solution at a volume ratio of 1:0.21-0.32, the pH value is adjusted to 4.5-4.7 with dilute nitric acid, refluxed for 60-70 minutes, washed with deionized water for 2-4 times, and then dried at 45-50° C. for 12-14 hours to obtain phosphine-based hydrotalcite.
[0012] The present invention is further configured as follows: the mass ratio of the zinc nitrate hexahydrate to the aluminum nitrate nonahydrate is 2.1-2.3:1.
[0013] The present invention is further configured as follows: the mass ratio of the sodium hydroxide to the sodium carbonate is 1:0.72-0.78.
[0014] The present invention is further configured as follows: the concentration of the sodium dihydrogen phosphate aqueous solution is 19-21%.
[0015] The present invention is further configured as follows: the preparation process of the functional filler is as follows:
[0016] The nano-polyvinyl chloride microspheres are placed in an ethanol aqueous solution with a concentration of 65-70% at a solid-liquid ratio of 0.02-0.08 g / mL, and ultrasonically dispersed for 20-30 minutes. Hexadecyltrimethylammonium bromide with a mass of 18-22% of the nano-polyvinyl chloride microspheres is added thereto, and stirred at 120-240 r / min for 40-50 minutes, and then ammonia water with a concentration of 24-26% is added thereto to obtain a solution A.
[0017] Put tetraethyl orthosilicate in anhydrous ethanol at a volume ratio of 1:22-26, and stir at 120-160 r / min for 20-30 min to obtain solution B;
[0018] Solution B is placed in solution A at a volume ratio of 1:0.05-0.12, and auxiliary materials of 2.2-5.2% by mass of solution A are added thereto, stirred for 22-24 hours at 22-24°C and 80-140 r / min, filtered, washed with anhydrous ethanol and deionized water for 2-4 times respectively, and then dried at 45-50°C for 14-16 hours to obtain a functional filler.
[0019] The present invention is further configured as follows: the amount of ammonia water added is 11-13% of the volume of the ethanol aqueous solution.
[0020] The present invention is further configured as follows: the preparation process of the auxiliary material is as follows:
[0021] Mix polydimethylsiloxane and nano zinc oxide at a mass ratio of 0.12 to 0.22:1 at 1400 to 1500 r / min for 40 to 50 minutes;
[0022] After the mixing is completed, the mixture is dried at 35-40°C for 24-30 hours to obtain the auxiliary material.
[0023] The present invention is further configured as follows: the antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.
[0024] The second aspect of the present invention: also provides a method for preparing the above-mentioned infrared thermal insulation film containing phosphine-based hydrotalcite, comprising the following steps:
[0025] Step 1, accurately weighing chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant, and putting chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant into a mixing equipment for mixing and stirring;
[0026] Step 2: After the mixture is evenly mixed, the mixture is transferred into a mixer and subjected to a refining process at a temperature of 160 to 180° C. until the film-forming surface is smooth and free of cracks;
[0027] Step 3: then transfer the opened mixture to a flat vulcanizer for pressure molding, and finally obtain an infrared thermal insulation film containing phosphine-based hydrotalcite; wherein the pressure of the pressure molding is 5-8MPa, the temperature is 150-160°C, and the vulcanization time is set to 30-50min.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] In the present invention, chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, diphenyl 2-ethylhexyl phosphate and antioxidant are used as raw materials. Chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, diphenyl 2-ethylhexyl phosphate and antioxidant are put into a mixing device for mixing and stirring. After being evenly mixed, the obtained mixture is transferred to a mixer for refining and processing until the film-forming surface is smooth and crack-free, and then the refining mixture is moved to a flat vulcanizer for pressure molding, and the final product is an infrared thermal insulation film containing phosphine-based hydrotalcite. The infrared thermal insulation film containing phosphine-based hydrotalcite prepared by the present invention not only has a significant absorption effect on infrared light, but also has excellent thermal insulation performance, effectively ensuring its quality. The infrared thermal insulation film containing phosphine-based hydrotalcite provided by the present invention and the preparation method thereof have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides an infrared thermal insulation film containing phosphine-based hydrotalcite, which is composed of the following raw materials in parts by weight: 20 parts of chlorinated polyethylene, 10 parts of phosphine-based hydrotalcite, 3 parts of functional filler, 3 parts of calcium zinc stabilizer, 2 parts of diphenyl 2-ethylhexyl phosphate and 2 parts of antioxidant.
[0033] In this embodiment, it should be noted that the chlorinated polyethylene was purchased from Shandong Yanggu Xiangtai Plastic Co., Ltd., and the calcium zinc stabilizer was purchased from Qingdao Gabet New Material Technology Co., Ltd.
[0034] The preparation process of phosphine-based hydrotalcite is as follows:
[0035] Evenly dispersing zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a first pre-formulated solution;
[0036] Evenly dispersing sodium hydroxide and sodium carbonate in deionized water to obtain a second solution;
[0037] The first pre-prepared liquid and the second pre-prepared liquid were added to water at 80°C and 1250 r / min in a volume ratio of 1:2, wherein the volume of the water was twice the sum of the volumes of the first pre-prepared liquid and the second pre-prepared liquid, and the mixture was kept warm and stirred for 60 minutes, and then placed in an oven at 88°C for 12 hours. After filtration, the mixture was washed twice with deionized water, and then dried at 45°C for 15 hours to obtain a base material;
[0038] The base material was dispersed in deionized water at a solid-liquid ratio of 0.22 g / mL to obtain a mixed solution, the mixed solution was mixed with a sodium dihydrogen phosphate aqueous solution at a volume ratio of 1:0.21, the pH was adjusted to 4.5 with dilute nitric acid, refluxed for 60 minutes, washed twice with deionized water, and then dried at 45°C for 12 hours to obtain phosphine-based hydrotalcite.
[0039] Furthermore, the mass ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 2.1:1.
[0040] The mass ratio of sodium hydroxide to sodium carbonate is 1:0.72.
[0041] The concentration of the sodium dihydrogen phosphate aqueous solution was 19%.
[0042] In addition, the preparation process of the functional filler is as follows:
[0043] The nano-polyvinyl chloride microspheres were placed in a 65% ethanol aqueous solution at a solid-liquid ratio of 0.02 g / mL, and ultrasonically dispersed for 20 to 30 minutes. Hexadecyltrimethylammonium bromide, which was 18% of the mass of the nano-polyvinyl chloride microspheres, was added thereto, and stirred at 120 r / min for 40 minutes. Then, ammonia water with a concentration of 24% was added thereto to obtain a solution A.
[0044] TEOS was placed in anhydrous ethanol at a volume ratio of 1:22 and stirred at 120 r / min for 20 min to obtain solution B.
[0045] Solution B was placed in solution A at a volume ratio of 1:0.05, and 2.2% of the mass of solution A was added with auxiliary materials. The mixture was stirred at 22°C and 80 r / min for 22 hours. After filtration, the mixture was washed twice with anhydrous ethanol and deionized water respectively, and then dried at 45°C for 14 hours to obtain a functional filler.
[0046] Furthermore, the amount of ammonia water added is 11% of the volume of the ethanol aqueous solution.
[0047] The preparation process of auxiliary materials is as follows:
[0048] Polydimethylsiloxane and nano zinc oxide were mixed at a mass ratio of 0.12:1 at 1400 r / min for 40 min;
[0049] After the mixing is completed, it is dried at 35°C for 24 hours to obtain the auxiliary material.
[0050] In this embodiment, it should be noted that the nano-polyvinyl chloride microspheres were purchased from Shaanxi Xingbei Aike Biotechnology Co., Ltd., and the nano-zinc oxide was purchased from Huzhou Mister New Materials Co., Ltd.
[0051] Among them, antioxidant 1010 is selected as the antioxidant.
[0052] In addition, this embodiment also provides a method for preparing the above-mentioned infrared thermal insulation film containing phosphine-based hydrotalcite, comprising the following steps:
[0053] Step 1, accurately weighing chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant, and putting chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant into a mixing equipment for mixing and stirring;
[0054] Step 2: After the mixture is evenly mixed, the mixture is transferred into a mixer and subjected to a mixing process at 160° C. until the film surface is smooth and free of cracks;
[0055] Step 3: The mixed mixture is then transferred to a flat-plate vulcanizer for pressure molding, and the final product is an infrared thermal insulation film containing phosphine-based hydrotalcite; wherein the pressure of the pressure molding is 5 MPa, the temperature is 150° C., and the vulcanization time is set to 30 min.
[0056] Example 2
[0057] The preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite provided in this embodiment is basically the same as that in Example 1, except that: the specific raw material composition and the specific preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite in this embodiment are different; the specific raw material composition and the specific preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite in this embodiment are as follows:
[0058] An infrared thermal insulation film containing phosphine-based hydrotalcite is composed of the following raw materials in parts by weight: 25 parts of chlorinated polyethylene, 12 parts of phosphine-based hydrotalcite, 4 parts of functional filler, 4 parts of calcium zinc stabilizer, 3 parts of diphenyl 2-ethylhexyl phosphate and 3 parts of antioxidant.
[0059] In this embodiment, it should be noted that the chlorinated polyethylene was purchased from Shandong Yanggu Xiangtai Plastic Co., Ltd., and the calcium zinc stabilizer was purchased from Qingdao Gabet New Material Technology Co., Ltd.
[0060] The preparation process of phosphine-based hydrotalcite is as follows:
[0061] Evenly dispersing zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a first pre-formulated solution;
[0062] Evenly dispersing sodium hydroxide and sodium carbonate in deionized water to obtain a second solution;
[0063] The first pre-prepared liquid and the second pre-prepared liquid were added to water at 85°C and 1350 r / min in a volume ratio of 1:3, wherein the volume of the water was 3 times the sum of the volumes of the first pre-prepared liquid and the second pre-prepared liquid, and the mixture was kept warm and stirred for 70 minutes, and then placed in an oven at 90°C for 13 hours. After filtration, the mixture was washed with deionized water for 3 times, and then dried at 47°C for 16 hours to obtain a base material;
[0064] The base material was dispersed in deionized water at a solid-liquid ratio of 0.25 g / mL to obtain a mixed solution, the mixed solution was mixed with a sodium dihydrogen phosphate aqueous solution at a volume ratio of 1:0.27, the pH was adjusted to 4.6 with dilute nitric acid, refluxed for 65 minutes, washed with deionized water for 3 times, and then dried at 47°C for 13 hours to obtain phosphine-based hydrotalcite.
[0065] Furthermore, the mass ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 2.2:1.
[0066] The mass ratio of sodium hydroxide to sodium carbonate is 1:0.75.
[0067] The concentration of the sodium dihydrogen phosphate aqueous solution is 20%.
[0068] In addition, the preparation process of the functional filler is as follows:
[0069] The nano-polyvinyl chloride microspheres were placed in a 67% ethanol aqueous solution at a solid-liquid ratio of 0.05 g / mL, and ultrasonically dispersed for 25 minutes. Hexadecyltrimethylammonium bromide, which was 20% of the mass of the nano-polyvinyl chloride microspheres, was added thereto, and stirred at 180 r / min for 45 minutes. Then, ammonia water with a concentration of 25% was added thereto to obtain a solution A.
[0070] TEOS was placed in anhydrous ethanol at a volume ratio of 1:24 and stirred at 140 r / min for 25 min to obtain solution B.
[0071] Solution B was placed in solution A at a volume ratio of 1:0.09, and 3.7% of the mass of solution A was added with auxiliary materials. The mixture was stirred at 23°C and 110 r / min for 23 hours. After filtration, the mixture was washed three times with anhydrous ethanol and deionized water respectively, and then dried at 47°C for 15 hours to obtain a functional filler.
[0072] Furthermore, the amount of ammonia water added is 12% of the volume of the ethanol aqueous solution.
[0073] The preparation process of auxiliary materials is as follows:
[0074] Polydimethylsiloxane and nano zinc oxide were mixed at a mass ratio of 0.17:1 at 1450 r / min for 45 min;
[0075] After the mixing is completed, it is dried at 37°C for 27 hours to obtain the auxiliary material.
[0076] In this embodiment, it should be noted that the nano-polyvinyl chloride microspheres were purchased from Shaanxi Xingbei Aike Biotechnology Co., Ltd., and the nano-zinc oxide was purchased from Huzhou Mister New Materials Co., Ltd.
[0077] Among them, antioxidant 1076 is selected as the antioxidant.
[0078] In addition, this embodiment also provides a method for preparing the above-mentioned infrared thermal insulation film containing phosphine-based hydrotalcite, comprising the following steps:
[0079] Step 1, accurately weighing chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant, and putting chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant into a mixing equipment for mixing and stirring;
[0080] Step 2: After the mixture is evenly mixed, the mixture is transferred into a mixer and subjected to a mixing process at a temperature of 170° C. until the film-forming surface is smooth and free of cracks;
[0081] Step 3: The mixed mixture is then transferred to a flat-plate vulcanizer for pressure molding, and the final product is an infrared thermal insulation film containing phosphine-based hydrotalcite; wherein the pressure of the pressure molding is 6 MPa, the temperature is 155° C., and the vulcanization time is set to 40 min.
[0082] Example 3
[0083] The preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite provided in this embodiment is basically the same as that in Example 1, except that: the specific raw material composition and the specific preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite in this embodiment are different; the specific raw material composition and the specific preparation method of the infrared thermal insulation film containing phosphine-based hydrotalcite in this embodiment are as follows:
[0084] An infrared thermal insulation film containing phosphine-based hydrotalcite is composed of the following raw materials in parts by weight: 30 parts of chlorinated polyethylene, 14 parts of phosphine-based hydrotalcite, 6 parts of functional filler, 6 parts of calcium zinc stabilizer, 3 parts of diphenyl 2-ethylhexyl phosphate and 5 parts of antioxidant.
[0085] In this embodiment, it should be noted that the chlorinated polyethylene was purchased from Shandong Yanggu Xiangtai Plastic Co., Ltd., and the calcium zinc stabilizer was purchased from Qingdao Gabet New Material Technology Co., Ltd.
[0086] The preparation process of phosphine-based hydrotalcite is as follows:
[0087] Evenly dispersing zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a first pre-formulated solution;
[0088] Evenly dispersing sodium hydroxide and sodium carbonate in deionized water to obtain a second solution;
[0089] The first pre-prepared liquid and the second pre-prepared liquid were added to water at 90°C and 1500 r / min in a volume ratio of 1:4, wherein the volume of the water was 3 times the sum of the volumes of the first pre-prepared liquid and the second pre-prepared liquid, and the mixture was kept warm and stirred for 80 minutes, and then kept in an oven at 92°C for 14 hours. After filtration, the mixture was washed with deionized water for 4 times, and then dried at 50°C for 17 hours to obtain a base material;
[0090] The base material was dispersed in deionized water at a solid-liquid ratio of 0.28 g / mL to obtain a mixed solution, the mixed solution was mixed with a sodium dihydrogen phosphate aqueous solution at a volume ratio of 1:0.32, the pH was adjusted to 4.7 with dilute nitric acid, refluxed for 70 minutes, washed with deionized water for 4 times, and then dried at 50°C for 14 hours to obtain phosphine-based hydrotalcite.
[0091] Furthermore, the mass ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 2.3:1.
[0092] The mass ratio of sodium hydroxide to sodium carbonate is 1:0.78.
[0093] The concentration of the sodium dihydrogen phosphate aqueous solution was 21%.
[0094] In addition, the preparation process of the functional filler is as follows:
[0095] The nano-polyvinyl chloride microspheres were placed in a 70% ethanol aqueous solution at a solid-liquid ratio of 0.08 g / mL, and ultrasonically dispersed for 30 minutes. Hexadecyltrimethylammonium bromide, which was 18-22% of the mass of the nano-polyvinyl chloride microspheres, was added thereto, and stirred at 240 r / min for 50 minutes. Then, ammonia water with a concentration of 26% was added thereto to obtain a solution A.
[0096] TEOS was placed in anhydrous ethanol at a volume ratio of 1:26 and stirred at 160 r / min for 30 min to obtain solution B.
[0097] Solution B was placed in solution A at a volume ratio of 1:0.12, and 5.2% of the mass of auxiliary materials of solution A were added thereto. The mixture was stirred at 24°C and 140 r / min for 24 hours. After filtration, the mixture was washed with anhydrous ethanol and deionized water for 4 times respectively, and then dried at 50°C for 16 hours to obtain a functional filler.
[0098] Furthermore, the amount of ammonia water added is 13% of the volume of the ethanol aqueous solution.
[0099] The preparation process of auxiliary materials is as follows:
[0100] Polydimethylsiloxane and nano zinc oxide were mixed at a mass ratio of 0.22:1 at 1500 r / min for 50 min;
[0101] After the mixing is completed, it is dried at 40°C for 30 hours to obtain an auxiliary material.
[0102] In this embodiment, it should be noted that the nano-polyvinyl chloride microspheres were purchased from Shaanxi Xingbei Aike Biotechnology Co., Ltd., and the nano-zinc oxide was purchased from Huzhou Mister New Materials Co., Ltd.
[0103] Among them, the antioxidant is antioxidant CA.
[0104] In addition, this embodiment also provides a method for preparing the above-mentioned infrared thermal insulation film containing phosphine-based hydrotalcite, comprising the following steps:
[0105] Step 1, accurately weighing chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant, and putting chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant into a mixing equipment for mixing and stirring;
[0106] Step 2: After the mixture is evenly mixed, the mixture is transferred into a mixer and subjected to a mixing process at 180° C. until the film surface is smooth and free of cracks;
[0107] Step 3: The mixed mixture is then transferred to a flat-plate vulcanizer for pressure molding, and the final product is an infrared thermal insulation film containing phosphine-based hydrotalcite; wherein the pressure of the pressure molding is 8 MPa, the temperature is 160° C., and the vulcanization time is set to 50 min.
[0108] Comparative Example 1: The difference from Example 1 is that in this example, an equal amount of commercially available hydrotalcite (purchased from Guangdong Xiaoda Chemical Co., Ltd.) is used to replace the phosphine-containing hydrotalcite.
[0109] Comparative Example 2: The difference from Example 1 is that this example does not contain functional fillers.
[0110] Performance test: The infrared thermal insulation film samples provided in Examples 1 to 3 and Comparative Examples 1 to 2 are marked as Examples 1 to 3 and Comparative Examples 1 to 2, respectively; and the relevant properties of the infrared thermal insulation films provided in Examples 1 to 3 and Comparative Examples 1 to 2 are tested as follows:
[0111] 1. Infrared light transmittance test: The test method is to use a spectrophotometer (Shimadzu, Japan, model: UV-3101PC) to test the light transmittance in the wavelength range of 400 to 600nm.
[0112] 2. Thermal insulation test: The test method is in accordance with the testing standard of GB / T3399-1982.
[0113] The obtained test data are recorded in Table 1 and Table 2 below:
[0114] Table 1 Infrared light transmittance test results of each group of infrared thermal insulation films
[0115] Group Light transmittance (%) Example 1 Group 34.5 Example 2 Group 33.6 Example 3 Group 34.1 Comparison group 1 65.8 Comparison of 2 groups 82.9
[0116] Table 2 Insulation test results of each group of infrared insulation films
[0117] Group Thermal conductivity (W / (m·K)) Example 1 Group 0.22 Example 2 Group 0.24 Example 3 Group 0.21 Comparison group 1 0.28 Comparison of 2 groups 0.35
[0118] By comparing and analyzing the relevant data in Table 1 and Table 2, it can be seen that the infrared thermal insulation film containing phosphine-based hydrotalcite prepared by the present invention not only has a significant absorption effect on infrared light, but also has excellent thermal insulation performance, effectively ensuring its quality. This shows that the infrared thermal insulation film containing phosphine-based hydrotalcite and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.
[0119] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0120] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An infrared thermal insulation film containing phosphine-based hydrotalcite, characterized in that: The invention is composed of the following raw materials in parts by weight: 20-30 parts of chlorinated polyethylene, 10-14 parts of phosphine-based hydrotalcite, 3-6 parts of functional fillers, 3-6 parts of calcium zinc stabilizers, 2-3 parts of diphenyl 2-ethylhexyl phosphate and 2-5 parts of antioxidants.
2. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 1, characterized in that: The preparation process of the phosphine-based hydrotalcite is as follows: Evenly dispersing zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a first pre-formulated solution; Evenly dispersing sodium hydroxide and sodium carbonate in deionized water to obtain a second solution; The first pre-prepared liquid and the second pre-prepared liquid are added to water at 80-90° C. and 1250-1500 r / min in a volume ratio of 1:2-4, wherein the volume of the water is 2-3 times the sum of the volumes of the first pre-prepared liquid and the second pre-prepared liquid, and the mixture is kept warm and stirred for 60-80 minutes, and then placed in an oven at a constant temperature of 88-92° C. for 12-14 hours, filtered, washed with deionized water for 2-4 times, and then dried at 45-50° C. for 15-17 hours to obtain a base material; The base material is dispersed in deionized water at a solid-liquid ratio of 0.22-0.28 g / mL to obtain a mixed solution, the mixed solution is mixed with a sodium dihydrogen phosphate aqueous solution at a volume ratio of 1:0.21-0.32, the pH value is adjusted to 4.5-4.7 with dilute nitric acid, refluxed for 60-70 minutes, washed with deionized water for 2-4 times, and then dried at 45-50° C. for 12-14 hours to obtain phosphine-based hydrotalcite.
3. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 2, characterized in that: The mass ratio of the zinc nitrate hexahydrate to the aluminum nitrate nonahydrate is 2.1-2.3:
1.
4. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 2, characterized in that: The mass ratio of the sodium hydroxide to the sodium carbonate is 1:0.72-0.
78.
5. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 2, characterized in that: The concentration of the sodium dihydrogen phosphate aqueous solution is 19-21%.
6. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 1, characterized in that: The preparation process of the functional filler is as follows: The nano-polyvinyl chloride microspheres are placed in an ethanol aqueous solution with a concentration of 65-70% at a solid-liquid ratio of 0.02-0.08 g / mL, and ultrasonically dispersed for 20-30 minutes. Hexadecyltrimethylammonium bromide with a mass of 18-22% of the nano-polyvinyl chloride microspheres is added thereto, and stirred at 120-240 r / min for 40-50 minutes, and then ammonia water with a concentration of 24-26% is added thereto to obtain a solution A. Put tetraethyl orthosilicate in anhydrous ethanol at a volume ratio of 1:22-26, and stir at 120-160 r / min for 20-30 min to obtain solution B; Solution B is placed in solution A at a volume ratio of 1:0.05-0.12, and auxiliary materials of 2.2-5.2% by mass of solution A are added thereto, stirred for 22-24 hours at 22-24°C and 80-140 r / min, filtered, washed with anhydrous ethanol and deionized water for 2-4 times respectively, and then dried at 45-50°C for 14-16 hours to obtain a functional filler.
7. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 6, characterized in that: The amount of ammonia water added is 11-13% of the volume of the ethanol aqueous solution.
8. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 6, characterized in that: The preparation process of the auxiliary material is as follows: Mix polydimethylsiloxane and nano zinc oxide at a mass ratio of 0.12 to 0.22:1 at 1400 to 1500 r / min for 40 to 50 minutes; After the mixing is completed, the mixture is dried at 35-40°C for 24-30 hours to obtain the auxiliary material.
9. The infrared thermal insulation film containing phosphine-based hydrotalcite according to claim 1, characterized in that: The antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.
10. The method for preparing an infrared thermal insulation film containing phosphine-based hydrotalcite according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1, accurately weighing chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant, and putting chlorinated polyethylene, phosphine-based hydrotalcite, functional filler, calcium zinc stabilizer, 2-ethylhexyl diphenyl phosphate and antioxidant into a mixing equipment for mixing and stirring; Step 2: After the mixture is evenly mixed, the mixture is transferred into a mixer and subjected to a refining process at a temperature of 160 to 180° C. until the film-forming surface is smooth and free of cracks; Step 3: then transfer the opened mixture to a flat vulcanizer for pressure molding, and finally obtain an infrared thermal insulation film containing phosphine-based hydrotalcite; wherein the pressure of the pressure molding is 5-8MPa, the temperature is 150-160°C, and the vulcanization time is set to 30-50min.
Citation Information
Patent Citations
Polyethylene film with infrared absorption function and preparation method of polyethylene film
CN103113654A
Preparation method of polymer / ZnO / SiO2 nano-composite microspheres
CN105837840A
Flexible medium and far-waveband infrared absorbing film and preparation method thereof
CN109507766A
Hydrotalcite compound process for producing the same, and agricirultural film containing the same
CN1289307A
Multifunctional layered object
CN201437574U