Blended elastomer for continuous shaping at body temperature and application
By using a blended structure of viscoelastic transform phase and thermoplastic/thermoset elastic phase in shape memory materials, the problem of shape mismatch at human body temperature is solved, continuous shaping and adaptive fit are achieved, and wearable comfort is improved and material strength, and high temperature self-healing and temperature display functions.
Patent Information
- Application Number
- CN202410934690.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-26
AI Technical Summary
Existing shape memory materials cannot be continuously shaped at human body temperature, resulting in shape mismatch, causing stress concentration and pain, and lack of sufficient strength and shape maintenance capabilities.
Using a blended structure of 30-50 parts by volume of viscoelastic transforming phase material and 50-70 parts by volume of thermoplastic/thermoset elastic phase material, the shape fixation is achieved under human body temperature through preheating and external force, and high viscosity is used. Elasticity causes creep to further fit the human body shape and restore the original shape at high temperature.
It realizes the fixed and slight deformation bonding of large-deformed shapes at 20-40℃, reduces stress concentration, has good elasticity and self-repairability, is suitable for different usage scenarios, and displays temperature information through color-changing crystals.
Smart Images

Figure HDA0004940937200000011 
Figure HDA0004940937200000012 
Figure HDA0004940937200000013
Abstract
Description
Technical Field
[0001] The invention relates to an elastomeric material and application, and in particular to a blended elastomer for continuous shaping at body temperature and application. Background Art
[0002] Shape memory polymers generally have two parts in structure: one part is the elastic phase; the other part is the transition (reversible) phase. The transition phase softens after being stimulated (such as heat, light, magnetism, electricity, etc.) and is used to fix the temporary shape, while the elastic phase is relatively stable and is used for shape recovery. By adjusting the two phases of the material, the material can be fixed in a temporary shape near human body temperature, and return to the original shape after heating again. It is often used in wearable products that fit the shape of various parts of the human body. A type of body temperature / room temperature plastic shape memory material (CN108192321A, CN106832940B) uses a highly elastic polymer material as the elastic phase, so that the blended material has excellent elasticity, and the specially selected transition phase material can make the blended material have heat-driven shape memory characteristics, and the addition of component materials can adjust the elastic properties and crystallization rate of the blended material. However, the limitation of this invention is that the material after the fixed temporary shape is determined cannot change its shape further, and the human body may have slight shape changes throughout the day, resulting in stress concentration, pain, or looseness due to insufficient matching, affecting the wearing experience.
[0003] In order to solve the problem of wearing comfort, there is a type of slow-rebound memory foam material (CN101298490A, CN103030782A, CN103937199A, CN104193954A). This type of material is mainly improved on the rapid rebound of ordinary sponges, and slowly recovers its original shape from room temperature to human body temperature, which can better solve the above-mentioned shape matching problem. However, this type of material lacks sufficient strength, and the temporary shape cannot be maintained. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a blended elastomer that can be continuously shaped at body temperature; it can fit the shape of the human body at 20-40°C to achieve large deformation shape fixation, and then use the creep caused by the high viscoelasticity of the material near body temperature to produce small deformations, further fit the shape of the human body to reduce stress concentration.
[0005] Technical solution: The blended elastomer for continuous shaping at body temperature described in the present invention includes 30-50 parts by volume of a viscoelastic transition phase material and 50-70 parts by volume of a thermoplastic / thermosetting elastic phase material, and is blended to form a blended elastomer; the blended elastomer conforms to the shape of the human body at 20-40°C after preheating, undergoes slight deformation under continuous external force at body temperature, and further conforms to the human body to reduce stress concentration; after separation from the human body, it is heated to a high temperature again and returns to its original shape; the preheating temperature and the high temperature temperature are 45-100°C; at 15-40°C, the elastic modulus of the blended elastomer is 0.1-100MPa.
[0006] Among them, the viscoelastic transition phase material is a viscoelastic thermoplastic / thermosetting polymer; the viscoelastic transition phase material is selected from at least one of polyurethane (TPU), polypropylene (PP), epoxy resin (ER), phenolic resin (PF), and urea-formaldehyde resin; the viscoelastic transition phase material has a softening temperature of 45-80°C, hardens at 15-40°C, has an elastic modulus of 1-250MPa at 15-40°C, and has a relaxation time of 2000-5000s under the Maxwell model at 30-40°C.
[0007] Wherein, the thermoplastic elastic phase material is thermoplastic elastic rubber; the thermoplastic elastic phase material is selected from at least one of styrene elastomers, olefin elastomers, diene elastomers, vinyl chloride elastomers, urethane elastomers (TPU), ester elastomers (TPEE), amide elastomers (TPAE), organic fluorine elastomers (TPF), ethylene vinyl acetate copolymers (EVA), silicone elastomers or ethylene elastomers; further, the styrene elastomer is at least one of SBS, SIS, SEBS, SEPS; the olefin elastomer is TPO and / or TPV; the diene elastomer is TPB and / or TPI; the vinyl chloride elastomer is TPVC and / or TCPE;
[0008] The melting temperature of the thermoplastic elastic phase material is 100-200° C., and the elastic modulus at 15-40° C. is 0.05-50 MPa.
[0009] Among them, the thermosetting elastic phase material is a single-component or two-component natural rubber and synthetic rubber, polyether urethane elastomer, epoxy elastomer, polyester elastomer, and acrylic elastomer; further, the single-component or two-component natural rubber and synthetic rubber is at least one of latex, nitrile rubber, mixed polyurethane, silicone, butyl rubber and chloroprene rubber; the crosslinking method of the thermosetting elastic phase material itself is room temperature crosslinking, heat crosslinking, light crosslinking, humidity crosslinking, and radiation crosslinking, and the elastic modulus at 15-40°C is 0.05-50MPa.
[0010] Among them, the thermosetting / thermoplastic elastic phase material is 50-70 parts by volume of a styrene elastomer, and further, the styrene elastomer is at least one of SBS, SIS, SEBS, and SEPS; the viscoelastic transition phase material is 30-50 parts by volume of a viscoelastic thermoplastic polyurethane, and the softening temperature of the material after blending is 45-80°C, and the elastic modulus at 15-40°C is 0.1-100MPa; the blended material is adaptively matched to shape by creep at 30-40°C, or is softened by heating and then shaped at 20-40°C, with a shape fixation rate of 60-99%, and a shape recovery rate after heating exceeding 90%.
[0011] Among them, the thermosetting / thermoplastic elastic phase material is 50-70 parts by volume of a single-component or two-component silicone rubber, the viscoelastic transition phase material is 30-50 parts by volume of a viscoelastic thermoplastic polyurethane, the softening temperature of the material after hardening and molding is 45-80°C, and the elastic modulus at 0-40°C is 0.1-100MPa; the hardened and molded material can be adaptively matched to shape by creep at 20-40°C, or can be shaped at 20-40°C after being softened by heating, the shape fixation rate is 60-99%, and the shape recovery rate after heating exceeds 95%.
[0012] Wherein, when the viscoelastic transition phase is a viscoelastic thermoplastic polymer and the elastic phase is a thermoplastic elastomer, the preparation method is: heating and melting the thermoplastic elastomer and the viscoelastic thermoplastic polymer by high-temperature blending and then uniformly mixing them, and then cooling and hardening them into a shape;
[0013] When the viscoelastic transition phase is a viscoelastic thermoplastic polymer and the elastic phase is a thermosetting elastomer, the preparation method is: heating corresponding volumes of a liquid pre-crosslinking single-component or two-component thermosetting elastomer and a viscoelastic thermoplastic polymer respectively and uniformly mixing them by high-temperature blending, and then curing and forming them by conventional crosslinking methods;
[0014] When the viscoelastic transition phase is a viscoelastic thermosetting polymer and the elastic phase is a thermoplastic elastomer, the preparation method is: heating the thermoplastic elastomer material and the viscoelastic thermosetting polymer powder particles in corresponding volumes and uniformly mixing them, and then cooling and hardening them into a shape;
[0015] When the viscoelastic transition phase is a viscoelastic thermosetting polymer and the elastic phase is a thermosetting elastomer, the preparation method is: mixing corresponding volumes of a single-component or two-component thermosetting elastomer with viscoelastic thermosetting polymer powder at room temperature, and then curing and molding by conventional cross-linking.
[0016] The self-healing property at high temperature means that after scratches / cracks appear on the material, the material can be heated to a softening temperature to close the scratches / cracks.
[0017] Among them, it also includes color-changing crystals that can change color near human body temperature for displaying the material temperature, thereby indicating the actual temperature of the material. The color of the color-changing crystals can change repeatedly with the temperature.
[0018] The use of the above-mentioned blended elastomer for continuous shaping at body temperature in the preparation of in-ear products.
[0019] Wherein, the in-ear product includes earphones and earplugs; the earphones include an earphone body, and the earphone body is provided with an in-ear part for inserting into the ear;
[0020] When the above-mentioned blended elastomer for continuous shaping at body temperature is used to prepare an in-ear part or an earplug, the in-ear part or the earplug is preheated and inserted into the ear near body temperature to be shaped to match the ear structure; after being taken out, the contour of the in-ear part or the earplug is maintained at room temperature, and after being inserted into the ear again, it can continuously creep at body temperature to match the ear structure.
[0021] The ear-entry part of the present invention includes the shape of the earphone head without elastic earphone plugs and the shape of the earphone head with elastic earphone plugs in the prior art; the earphone plugs have inner holes for installation in the earphone head and plugging into the ear. The blended elastomer of the present invention can be used to prepare earphone heads without earphone plugs, and can also be used to prepare earphone plugs installed on earphone heads.
[0022] The earplug described in the present invention refers to an earplug without electronic components that can be directly inserted into the ear for use, such as a noise reduction earplug.
[0023] Wherein, the preheating shaping and creep matching at body temperature can be repeated.
[0024] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects: (1) The blended elastomer of the present invention can be preheated to fit the shape of the human body at 20-40°C, achieving large deformation and shape fixation, and then using the creep caused by the high viscoelasticity of the material near body temperature to produce small deformation, achieving further fit in real time and reducing stress concentration; after separation from the human body, the viscoelasticity decreases at room temperature, and there is no obvious shape change in the free state; after being heated to a high temperature again, it returns to its original shape; (2) The blended elastomer has good elasticity, and the stress and strain of the elastomer are basically consistent during cyclic loading, indicating that it is It will not deform or fail during repeated loading; (3) By selecting materials and adjusting the ratio of the transition phase to the elastic phase, the blended elastomer can have different moduli and hardnesses, which are suitable for different usage scenarios and provide effective support to prevent it from falling off during fitting with the human body; (4) The blended elastomer has self-healing properties at high temperatures. After scratches / cracks appear on the material, it can be heated to the softening temperature to quickly close the scratches / cracks; (5) The blended elastomer displays the material temperature by adding color-changing crystals that can change color near human body temperature, which is used to indicate the actual temperature of the material. Its color can change repeatedly with temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The stress relaxation of the viscoelastic thermoplastic polyurethane of the transition phase material of Example 1 at (a) small deformation and (b) large deformation at room temperature and near body temperature;
[0026] Figure 2 The cyclic loading curve of the viscoelastic thermoplastic polyurethane of the transition phase material at room temperature of Example 1;
[0027] Figure 3 The stress relaxation of the thermoplastic elastic rubber of the elastic phase material of Example 1 at (a) small deformation and (b) large deformation at room temperature and near body temperature;
[0028] Figure 4 The cyclic loading curve of the thermoplastic elastic rubber of the elastic phase material of Example 1 at room temperature;
[0029] Figure 5 The stress relaxation of the blended elastomer of Example 1 at (a) small deformation and (b) large deformation at room temperature and near body temperature;
[0030] Figure 6 This is the cyclic loading curve at room temperature of the blended elastomer for continuous shaping at body temperature of Example 1. DETAILED DESCRIPTION
[0031] The present invention is described in further detail below.
[0032] Example 1
[0033] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a styrene-based thermoplastic elastomer TPR0A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with an elastic modulus of 0.07MPa and 60 parts by volume; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), with an elastic modulus of 1.45MPa and 40 parts by volume.
[0034] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them uniformly mixed; (2) pouring them into a mold; and (3) cooling them to room temperature and hardening them to obtain a blended elastomer for continuous shaping at body temperature.
[0035] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 98%, the recovery rate is 97%, and the elastic modulus is 0.15 MPa.
[0036] Example 2
[0037] The difference between this embodiment and embodiment 1 is that the volume fraction of the elastic phase material used is 65 parts, and the volume fraction of the transition phase material used is 35 parts.
[0038] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 90%, the recovery rate is 98%, and the elastic modulus is 0.11 MPa.
[0039] Example 3
[0040] The difference between this embodiment and embodiment 1 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0041] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 85%, the recovery rate is 99%, and the elastic modulus is 0.08 MPa.
[0042] Example 4
[0043] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a styrene thermoplastic elastomer TPR10A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with an elastic modulus of 0.5 MPa and 60 parts by volume; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), with an elastic modulus of 1.45 MPa and 40 parts by volume.
[0044] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them uniformly mixed; (2) pouring them into a mold; and (3) cooling them to room temperature and hardening them to obtain a blended elastomer for continuous shaping at body temperature.
[0045] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 90%, the recovery rate is 97%, and the elastic modulus is 0.7 MPa.
[0046] Example 5
[0047] The difference between this embodiment and embodiment 4 is that the volume fraction of the elastic phase material used is 65 parts, and the volume fraction of the transition phase material used is 35 parts.
[0048] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 89%, the recovery rate is 98%, and the elastic modulus is 0.65 MPa.
[0049] Example 6
[0050] The difference between this embodiment and embodiment 4 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0051] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 81%, the recovery rate is 99%, and the elastic modulus is 0.6 MPa.
[0052] Example 7
[0053] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E610 thermosetting two-component rubber produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinking agent B, the crosslinking curing type is thermal crosslinking curing, the elastic modulus is 0.18 MPa, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 1.45 MPa, and the volume fraction is 40.
[0054] The preparation method is as follows: (1) respectively mixing corresponding volumes of a rubber matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling to 25°C and mixing the matrix with the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 25°C for 6 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0055] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 95%, the recovery rate is 100%, and the elastic modulus is 0.35 MPa.
[0056] Example 8
[0057] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E610 thermosetting two-component rubber produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinking agent B, the crosslinking curing type is thermal crosslinking curing, the elastic modulus is 0.18 MPa, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 1.45 MPa, and the volume fraction is 40.
[0058] The preparation method is as follows: (1) respectively mixing corresponding volumes of a rubber matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling to 20°C and mixing the matrix with the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 120°C for 2 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0059] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 95%, the recovery rate is 100%, and the elastic modulus is 0.35 MPa.
[0060] Example 9
[0061] The difference between this embodiment and embodiment 7 is that the volume fraction of the elastic phase material used is 65 parts and the volume fraction of the transition phase material used is 35 parts.
[0062] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 89%, the recovery rate is 100%, and the elastic modulus is 0.26 MPa.
[0063] Example 10
[0064] The difference between this embodiment and embodiment 7 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0065] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 83%, the recovery rate is 100%, and the elastic modulus is 0.21 MPa.
[0066] Embodiment 11
[0067] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E640 thermosetting two-component rubber produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinking agent B, the crosslinking curing type is thermal crosslinking curing, the elastic modulus is 0.75 MPa, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 1.45 MPa, and the volume fraction is 40.
[0068] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silicone matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling to 25°C and mixing the matrix with the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 25°C for 6 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0069] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 90%, the recovery rate is 100%, and the elastic modulus is 0.9 MPa.
[0070] Example 12
[0071] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E640 thermosetting two-component rubber produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinking agent B, the crosslinking curing type is thermal crosslinking curing, the elastic modulus is 0.75 MPa, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 1.45 MPa, and the volume fraction is 40.
[0072] The preparation method is as follows: (1) respectively mixing corresponding volumes of a rubber matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling to 20°C and mixing the matrix with the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 120°C for 2 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0073] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 90%, the recovery rate is 100%, and the elastic modulus is 0.9 MPa.
[0074] Embodiment 13
[0075] The difference between this embodiment and embodiment 11 is that the volume fraction of the elastic phase material used is 65 parts and the volume fraction of the transition phase material used is 35 parts.
[0076] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 87%, the recovery rate is 100%, and the elastic modulus is 0.85 MPa.
[0077] Embodiment 14
[0078] The difference between this embodiment and embodiment 11 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0079] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 81%, the recovery rate is 100%, and the elastic modulus is 0.81 MPa.
[0080] Embodiment 15
[0081] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a thermosetting single-component rubber, the cross-linking curing type is thermal cross-linking curing, the elastic modulus is 0.5MPa, and the volume fraction is 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU) powder with a particle size of 10-100μm, the elastic modulus is 1.45MPa, and the volume fraction is 40.
[0082] The preparation method is as follows: (1) stirring the corresponding volume parts of the rubber component and the 10-100 μm viscoelastic thermosetting polyurethane powder at room temperature to make them uniformly mixed; (2) pouring into a mold; and (3) cross-linking and curing at a high temperature of 120°C to obtain a blended elastomer for continuous shaping at body temperature.
[0083] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 90%, the recovery rate is 100%, and the elastic modulus is 0.74 MPa.
[0084] Example 16
[0085] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a thermosetting single-component rubber, the cross-linking curing type is photo-cross-linking curing, the elastic modulus is 1.2MPa, and the volume fraction is 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 5MPa, and the volume fraction is 40.
[0086] The preparation method is as follows: (1) stirring the corresponding volume parts of the silicone component and the viscoelastic thermoplastic polyurethane at 120°C to make them uniformly mixed; (2) pouring them into a mold; and (3) cross-linking and curing them under 405nm UV light to obtain a blended elastomer for continuous shaping at body temperature.
[0087] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 89%, the recovery rate is 100%, and the elastic modulus is 2.3 MPa.
[0088] Embodiment 17
[0089] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a thermosetting single-component rubber, the cross-linking curing type is moisture cross-linking curing, the elastic modulus is 0.6MPa, and the volume fraction is 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 5MPa, and the volume fraction is 40.
[0090] The preparation method is as follows: (1) stirring the corresponding volume parts of the rubber component and the viscoelastic thermoplastic polyurethane at 120°C to make them uniformly mixed; (2) pouring them into a mold; and (3) cross-linking and curing them under the action of room temperature moisture to obtain a blended elastomer for continuous shaping at body temperature.
[0091] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 95%, the recovery rate is 100%, and the elastic modulus is 1.7 MPa.
[0092] Embodiment 18
[0093] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a thermosetting single-component rubber, the cross-linking curing type is radiation cross-linking curing, the elastic modulus is 5.3MPa, and the volume fraction is 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 12MPa, and the volume fraction is 40.
[0094] The preparation method is as follows: (1) fully stirring the rubber component and viscoelastic thermoplastic polyurethane in corresponding volumes at 100° C. to make them uniformly mixed; (2) pouring them into a mold; and (3) cross-linking and curing them under the rays of a radiation source to obtain a blended elastomer for continuous shaping at body temperature.
[0095] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 87%, the recovery rate is 100%, and the elastic modulus is 8.3 MPa.
[0096] Embodiment 19
[0097] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is a styrene thermoplastic elastomer TPR10A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with an elastic modulus of 0.5 MPa and 60 parts by volume; the transition phase material is a viscoelastic thermosetting polyurethane (TPU) powder with a particle size of 10-100 μm, an elastic modulus of 20 MPa, and 40 parts by volume.
[0098] The preparation method is as follows: (1) stirring the corresponding volume parts of styrene-based thermoplastic elastomer and 10-100 μm viscoelastic thermosetting polyurethane powder at 180° C. to make them uniformly mixed; (2) pouring them into a mold; and (3) cooling to room temperature and hardening them to obtain a blended elastomer for continuous shaping at body temperature.
[0099] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 98%, the recovery rate is 85%, and the elastic modulus is 3.5 MPa.
[0100] Embodiment 20
[0101] The difference between this embodiment and Embodiment 19 is that the volume fraction of the elastic phase material used is 65 parts and the volume fraction of the transition phase material used is 35 parts.
[0102] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 87%, the recovery rate is 90%, and the elastic modulus is 2.2 MPa.
[0103] Embodiment 21
[0104] The difference between this embodiment and Embodiment 19 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0105] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 80%, the recovery rate is 93%, and the elastic modulus is 1.5 MPa.
[0106] Embodiment 22
[0107] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E610 thermosetting two-component silicone produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinker B, with an elastic modulus of 0.18 MPa and 60 parts by volume; the transition phase material is viscoelastic thermosetting polyurethane (TPU) powder with a particle size of 10-100 μm, an elastic modulus of 20 MPa and 40 parts by volume.
[0108] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinking agent B with 10-100 μm viscoelastic thermosetting polyurethane powder particles at room temperature and stirring them thoroughly to make them uniformly mixed; (2) mixing the matrix and the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 25°C for 6 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0109] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 98%, the recovery rate is 90%, and the elastic modulus is 2.3 MPa.
[0110] Embodiment 23
[0111] A blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material is HY-E610 thermosetting two-component silicone produced by Shenzhen Hongyejie Technology Co., Ltd., including a matrix A and a crosslinker B, with an elastic modulus of 0.18 MPa and 60 parts by volume; the transition phase material is viscoelastic thermosetting polyurethane (TPU) powder with a particle size of 10-100 μm, an elastic modulus of 20 MPa and 40 parts by volume.
[0112] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinking agent B with 10-100 μm viscoelastic thermosetting polyurethane powder particles at room temperature and stirring them thoroughly to make them uniformly mixed; (2) mixing the matrix and the crosslinking agent; (3) pouring them into a mold; and (4) crosslinking and curing at 120°C for 2 hours to obtain a blended elastomer for continuous shaping at body temperature.
[0113] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 98%, the recovery rate is 90%, and the elastic modulus is 2.3 MPa.
[0114] Embodiment 24
[0115] The difference between this embodiment and embodiment 23 is that the volume fraction of the elastic phase material used is 65 parts and the volume fraction of the transition phase material used is 35 parts.
[0116] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 89%, the recovery rate is 92%, and the elastic modulus is 1.6 MPa.
[0117] Embodiment 25
[0118] The difference between this embodiment and embodiment 23 is that the volume fraction of the elastic phase material used is 70 parts and the volume fraction of the transition phase material used is 30 parts.
[0119] The shape fixation rate of the blended elastomer for continuous shaping at body temperature obtained in this embodiment is 81%, the recovery rate is 96%, and the elastic modulus is 0.85 MPa.
[0120] Embodiment 26
[0121] An earphone includes an earphone body, and the earphone body is provided with an ear inlet. The ear inlet of this embodiment simulates the shape of the earphone head without an elastic earphone plug in the prior art, and can be directly plugged into the ear; the ear inlet is called an earphone jacket. The earphone jacket of this embodiment is prepared from a blended elastomer for continuous shaping at body temperature. The elastic phase polymer material of the blended elastomer is a styrene-based thermoplastic elastomer TPR0A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with a volume fraction of 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), with an elastic modulus of 1.45MPa and a volume fraction of 40.
[0122] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them evenly mixed; (2) injecting the liquid blend into an earphone cover mold at an injection molding pressure of 3 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earphone cover that can be continuously shaped at body temperature.
[0123] The shape fixing rate of the earphone cover which is continuously reshaped at body temperature obtained in this embodiment reaches 98%, and the recovery rate reaches 97%.
[0124] Embodiment 27
[0125] On the basis of Example 26, different from Example 26, the elastic phase polymer material of the blended elastomer used in the earphone cover is styrene-based thermoplastic elastomer TPR10A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with a volume fraction of 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0126] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them evenly mixed; (2) injecting the liquid blend into an earphone cover mold at an injection molding pressure of 5 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earphone cover that can be continuously shaped at body temperature.
[0127] The shape fixing rate of the earphone cover which is continuously reshaped at body temperature obtained in this embodiment reaches 96%, and the recovery rate reaches 98%.
[0128] Embodiment 28
[0129] On the basis of Example 26, different from Example 26, the elastic phase polymer material in the components of the blended elastomer used in the earphone cover is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E610 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0130] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinker B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling the matrix to 25°C and mixing the matrix with the crosslinker; (3) injecting the liquid blend into an earphone jacket mold at an injection molding pressure of 3 MPa; (4) crosslinking and curing at 25°C for 6 hours to obtain an earphone jacket that can be continuously shaped at body temperature.
[0131] The shape fixing rate of the earphone cover which is continuously reshaped at body temperature obtained in this embodiment reaches 95%, and the recovery rate reaches 100%.
[0132] Embodiment 29
[0133] On the basis of Example 26, different from Example 26, the elastic phase polymer material in the components of the blended elastomer used in the earphone cover is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E640 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0134] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling the matrix to 20°C and mixing the matrix with the crosslinking agent; (3) injecting the liquid blend into an earphone jacket mold at an injection molding pressure of 5 MPa; (4) crosslinking and curing at 120°C for 2 hours to obtain an earphone jacket that can be continuously shaped at body temperature.
[0135] The shape fixing rate of the earphone cover which is continuously shaped at body temperature obtained in this embodiment reaches 92%, and the recovery rate reaches 100%.
[0136] Embodiment 30
[0137] An earplug without electronic components, which is used to be directly inserted into the ear; the earplug is prepared from a blended elastomer for continuous shaping at body temperature, wherein the elastic phase polymer material of the blended elastomer is a styrene-based thermoplastic elastomer TPR0A produced by Nanjing Hongxing New Materials Technology Co., Ltd., with a volume fraction of 60; the transition phase material is a viscoelastic thermoplastic polyurethane (TPU), with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0138] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them uniformly mixed; (2) injecting the liquid blend into an earplug mold at an injection molding pressure of 3 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earplug that can be continuously shaped at body temperature.
[0139] The shape fixation rate of the earplug that is continuously reshaped at body temperature obtained in this embodiment is 98%, and the recovery rate is 97%.
[0140] Embodiment 31
[0141] On the basis of Example 30, different from Example 30, the elastic phase polymer material of the blended elastomer used in the earplug is styrene-based thermoplastic elastomer TPR10A produced by Nanjing Hongxing New Material Technology Co., Ltd., with a volume fraction of 60 parts; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40 parts.
[0142] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them uniformly mixed; (2) injecting the liquid blend into an earplug mold at an injection molding pressure of 5 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earplug that can be continuously shaped at body temperature.
[0143] The shape fixation rate of the earplug that is continuously reshaped at body temperature obtained in this embodiment is 96%, and the recovery rate is 98%.
[0144] Embodiment 32
[0145] On the basis of Example 30, different from Example 30, the elastic phase polymer material in the components of the blended elastomer used in the earplug is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E610 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), and the elastic modulus is 1.45 MPa, and the volume fraction is 40.
[0146] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling the matrix to 25°C and mixing the matrix with the crosslinking agent; (3) injecting the liquid blend into an earplug mold at an injection molding pressure of 3 MPa; (4) crosslinking and curing at 25°C for 6 hours to obtain an earplug that can be continuously shaped at body temperature.
[0147] The shape fixation rate of the earplug that is continuously shaped at body temperature obtained in this embodiment reaches 95%, and the recovery rate reaches 100%.
[0148] Embodiment 33
[0149] On the basis of Example 30, different from Example 30, the elastic phase polymer material in the components of the blended elastomer used in the earplug is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E640 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, produced from, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU), the elastic modulus is 1.45MPa, and the volume fraction is 40.
[0150] The preparation method is as follows: (1) respectively mixing corresponding volumes of a silica gel matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniform; (2) cooling the matrix to 20°C and mixing the matrix with the crosslinking agent; (3) injecting the liquid blend into an earplug mold at an injection molding pressure of 5 MPa; (4) crosslinking and curing at 120°C for 2 hours to obtain an earplug that can be continuously shaped at body temperature.
[0151] The shape fixation rate of the earplug that is continuously shaped at body temperature obtained in this embodiment is 92%, and the recovery rate is 100%.
[0152] Embodiment 34
[0153] An earphone with electronic components includes an earphone body, the earphone body is provided with an earphone inlet, the earphone inlet is provided with an earphone plug, the earphone inlet of this embodiment simulates the shape of an earphone head with an elastic earphone plug in the prior art, and the earphone plug is equivalent to the earphone plug of the earphone head in the prior art. The earphone plug of this embodiment is prepared from a blended elastomer for continuous shaping at body temperature, and the elastic phase polymer material of the blended elastomer is selected from styrene thermoplastic elastomer TPR0A, produced by Nanjing Hongxing New Materials Technology Co., Ltd., with a volume fraction of 60; the transition phase material is selected from viscoelastic thermoplastic polyurethane (TPU), with an elastic modulus of 1.45MPa, and a volume fraction of 40.
[0154] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them evenly mixed; (2) injecting the liquid blend into an earphone plug mold at an injection molding pressure of 3 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earphone plug that continues to be shaped at body temperature.
[0155] The earphone plug that is continuously shaped at body temperature obtained in this embodiment has a shape fixing rate of 98% and a recovery rate of 97%.
[0156] Embodiment 35
[0157] On the basis of Example 34, different from Example 34, the elastic phase polymer material of the blended elastomer used in the earphone plug is styrene-based thermoplastic elastomer TPR10A produced by Nanjing Hongxing New Material Technology Co., Ltd., with a volume fraction of 60 parts; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40 parts.
[0158] The preparation method is as follows: (1) melting corresponding volumes of styrene-based thermoplastic elastomer and viscoelastic thermoplastic polyurethane at 180°C and stirring them thoroughly to make them evenly mixed; (2) injecting the liquid blend into an earphone plug mold at an injection molding pressure of 5 MPa; (3) cooling to room temperature and hardening the mixture to obtain an earphone plug that continues to be shaped at body temperature.
[0159] The shape fixation rate of the earphone plug that is continuously shaped at body temperature obtained in this embodiment is 96%, and the recovery rate is 98%.
[0160] Embodiment 36
[0161] On the basis of Example 34, different from Example 34, the elastic phase polymer material in the components of the blended elastomer used in the earphone plug is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E610 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0162] The preparation method is as follows: (1) respectively mixing corresponding volumes of a rubber matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling the matrix to 25°C and mixing the matrix with the crosslinking agent; (3) injecting the liquid blend into an earphone plug mold at an injection molding pressure of 3 MPa; (4) crosslinking and curing at 25°C for 6 hours to obtain an earphone plug that can be continuously shaped at body temperature.
[0163] The shape fixation rate of the earphone plug that is continuously shaped at body temperature obtained in this embodiment reaches 95%, and the recovery rate reaches 100%.
[0164] Embodiment 37
[0165] On the basis of Example 34, different from Example 34, the elastic phase polymer material in the components of the blended elastomer used in the earphone plug is selected from Shenzhen Hongyejie Technology Co., Ltd. HY-E640 thermosetting two-component rubber, including matrix A and cross-linking agent B, the cross-linking curing type is thermal cross-linking curing, and the volume fraction is 60; the transition phase material is viscoelastic thermoplastic polyurethane (TPU) with an elastic modulus of 1.45 MPa and a volume fraction of 40.
[0166] The preparation method is as follows: (1) respectively mixing corresponding volumes of a rubber matrix A and a crosslinking agent B with viscoelastic thermoplastic polyurethane at 120°C and stirring them thoroughly to make them uniformly mixed; (2) cooling the matrix to 20°C and mixing the matrix with the crosslinking agent; (3) injecting the liquid blend into an earphone plug mold at an injection molding pressure of 5 MPa; (4) crosslinking and curing at 120°C for 2 hours to obtain an earphone plug that can be continuously shaped at body temperature.
[0167] The shape fixation rate of the earphone plug that is continuously shaped at body temperature obtained in this embodiment reaches 92%, and the recovery rate reaches 100%.
[0168] Figure 1 Stress relaxation of the transition phase viscoelastic thermoplastic polyurethane of Example 1 at (a) 30% strain and (b) 80% strain at room temperature 25°C and body temperature 35°C.
[0169] Figure 2 The cyclic loading curve of the transition phase viscoelastic thermoplastic polyurethane at room temperature 25°C of Example 1, wherein the loading strain rate is 5×10-3 / s.
[0170] Figure 3 The stress relaxation of the elastic phase thermoplastic elastic rubber of Example 1 at (a) 30% strain and (b) 80% strain at room temperature 25°C and body temperature 35°C.
[0171] Figure 4 is the cyclic loading curve of the elastic phase thermoplastic elastic rubber of Example 1 at room temperature 25°C, wherein the loading strain rate is 5×10 -3 / s.
[0172] Figure 5 The stress relaxation of the blended elastomer of Example 1 at (a) 30% strain and (b) 80% strain near room temperature 25°C and body temperature 35°C; the volume of the elastic part of the blended elastomer is 60%; it can be seen that the relaxation effect of the elastomer near human body temperature is more obvious, which further fits the body shape and reduces stress concentration; after separation from the human body, the viscoelasticity is reduced at room temperature, and there is no obvious shape change in the free state; after heating to a high temperature again, it returns to its original shape.
[0173] Figure 6 The cyclic loading curve of the blended elastomer for continuous shaping at body temperature at room temperature 25°C of Example 1, wherein the loading strain rate is 5×10 -3 / s, the volume ratio of the elastic part of the blended elastomer is 60%; it can be seen that the blended elastomer has good elasticity, and the stress and strain of the elastomer are basically consistent during cyclic loading, indicating that it will not deform and fail during repeated loading.
Claims
1. A blended elastomer for continuous shaping at body temperature, characterized in that: The invention comprises 30-50 parts by volume of a viscoelastic transition phase material and 50-70 parts by volume of a thermoplastic / thermosetting elastic phase material, which are blended to form a blended elastomer; the blended elastomer conforms to the shape of the human body at 20-40°C after preheating, undergoes slight deformation under continuous external force at body temperature, and further conforms to the human body to reduce stress concentration; after being separated from the human body, the blended elastomer is heated to a high temperature again and returns to its original shape; the preheating temperature and the high temperature temperature are 45-100°C; at 15-40°C, the elastic modulus of the blended elastomer is 0.1-100MPa.
2. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: The viscoelastic transition phase material is a viscoelastic thermoplastic / thermosetting polymer; the viscoelastic transition phase material is selected from at least one of polyurethane, polypropylene, epoxy resin, phenolic resin, and urea-formaldehyde resin; the viscoelastic transition phase material has a softening temperature of 45-80°C, hardens at 15-40°C, has an elastic modulus of 1-250MPa at 15-40°C, and has a relaxation time of 2000-5000s under the Maxwell model at 30-40°C.
3. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: The thermoplastic elastic phase material is a thermoplastic elastic rubber; the thermoplastic elastic phase material is selected from at least one of styrene elastomers, olefin elastomers, diene elastomers, vinyl chloride elastomers, urethane elastomers, ester elastomers, amide elastomers, organic fluorine elastomers, ethylene vinyl acetate copolymers, silicone elastomers, and ethylene elastomers; the melting temperature of the thermoplastic elastic phase material is 100-200°C, and the elastic modulus at 15-40°C is 0.05-50MPa.
4. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: The thermosetting elastic phase material is selected from at least one of single-component or two-component natural rubber or synthetic rubber, polyether urethane elastomer, epoxy elastomer, polyester elastomer, and acrylic elastomer; the crosslinking method of the thermosetting elastic phase material itself is room temperature crosslinking, heat crosslinking, light crosslinking, humidity crosslinking, and radiation crosslinking, and the elastic modulus at 15-40°C is 0.05-50MPa.
5. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: The thermosetting / thermoplastic elastic phase material is 50-70 parts by volume of a styrene elastomer, and the viscoelastic transition phase material is 30-50 parts by volume of a viscoelastic thermoplastic polyurethane. The softening temperature of the blended elastomer after blending is 45-80°C, and the elastic modulus at 15-40°C is 0.1-100MPa; the blended elastomer matches the shape through creep adaptive adaptation at 30-40°C, or is shaped at 20-40°C after being softened by heating, and the shape fixation rate is 60-99%, and the shape recovery rate after heating exceeds 90%.
6. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: The thermosetting / thermoplastic elastic phase material is 50-70 parts by volume of a single-component or two-component silicone rubber, the viscoelastic transition phase material is 30-50 parts by volume of a viscoelastic thermoplastic polyurethane, the softening temperature of the material after hardening and molding is 45-80°C, and the elastic modulus at 0-40°C is 0.1-100MPa; the hardened and molded material can adaptively match the shape through creep at 20-40°C, or be shaped at 20-40°C after being softened by heating, the shape fixation rate is 60-99%, and the shape recovery rate after heating exceeds 95%.
7. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: When the viscoelastic transition phase is a viscoelastic thermoplastic polymer and the elastic phase is a thermoplastic elastomer, the preparation method of the blended elastomer is: heating and melting the thermoplastic elastomer and the viscoelastic thermoplastic polymer by high temperature blending and then uniformly mixing them, and then cooling and hardening them into a shape; When the viscoelastic transition phase is a viscoelastic thermoplastic polymer and the elastic phase is a thermosetting elastomer, the preparation method of the blended elastomer is: heating corresponding volumes of a liquid pre-crosslinking single-component or two-component thermosetting elastomer and a viscoelastic thermoplastic polymer respectively and uniformly mixing them by high-temperature blending, and then crosslinking and curing to form; When the viscoelastic transition phase is a viscoelastic thermosetting polymer and the elastic phase is a thermoplastic elastomer, the preparation method of the blended elastomer is: heating the thermoplastic elastomer material and the viscoelastic thermosetting polymer powder particles in corresponding volumes and uniformly mixing them, and then cooling and hardening them into a shape; When the viscoelastic transition phase is a viscoelastic thermosetting polymer and the elastic phase is a thermosetting elastomer, the preparation method of the blended elastomer is: blending corresponding volumes of a single-component or two-component thermosetting elastomer with viscoelastic thermosetting polymer powder at room temperature, followed by cross-linking and curing to form the blended elastomer.
8. The blended elastomer for continuous shaping at body temperature according to claim 1, characterized in that: It also includes a color-changing crystal for displaying the temperature of the material and can change color with the body temperature. The color-changing crystal can indicate the actual temperature of the material, and the color of the color-changing crystal can change repeatedly with the temperature.
9. Use of the blended elastomer for continuous shaping at body temperature as claimed in claim 1 in the preparation of in-ear products.
10. The use according to claim 9, characterized in that: The in-ear product includes earphones and earplugs; the earphones include an earphone body, and the earphone body is provided with an in-ear part for inserting into the ear; When the blended elastomer for continuous shaping at body temperature described in claim 1 is used to prepare an in-ear part or an earplug, the in-ear part or the earplug is preheated and inserted into the ear near body temperature to be shaped to match the ear structure; after being taken out, the contour of the in-ear part or the earplug is maintained at room temperature, and after being inserted into the ear again, it can continuously creep at body temperature to match the ear structure.