TPE (thermoplastic elastomer) odor-free spliced floor and production process thereof
By using raw materials such as sulfonic acid-based porous fillers and bisphenol A-type epoxy resins in TPE elastic floors, a composite resin with gas adsorption capacity is formed, and combined with inorganic fillers and flame retardants, the problem of harmful gases emitted by TPE elastic floors is solved. It achieves the effects of odor, wear resistance, antibacterial and flame retardant, and is suitable for installation in indoor places.
Patent Information
- Application Number
- CN202411008411.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing TPE elastic floor will emit harmful gases during use and cannot effectively solve the odor problem.
Using composite resins, the porous filler with gas adsorption capacity, the raw materials such as sulfonic acid-based porous filler, bisphenol A type epoxy resin and (3-mercaptopropyl) trimethoxysilane, etc., is formed by ultrasonic dispersion and reaction grafting, and the porous filler with gas adsorption capacity is combined with Inorganic fillers, flame retardants and antibacterial agents are used to prepare TPE clean-flavored assembled floors and vulcanize them through specific production processes.
The produced TPE odor assembly floor has good wear resistance, antibacterial properties and flame retardancy. It can effectively absorb internal gases, reduce odor emission, and is convenient to install. It is suitable for indoor places.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermoplastic floors, and in particular relates to a TPE odor-free assembled floor and a production process thereof. Background Art
[0002] In recent years, with the continuous improvement of public safety and environmental protection requirements, the demand for environmentally friendly flame-retardant indoor floor decoration materials suitable for large public places has become increasingly prominent. Rubber flooring has the characteristics of wear resistance, anti-slip, oil resistance, chemical corrosion resistance, bright colors, strong load-bearing capacity, easy installation and maintenance, and comfortable feeling on the feet. However, rubber flooring and bonding glue will emit harmful gases, which will be absorbed by people when used indoors, causing great harm to the human body.
[0003] Patent CN110066436A discloses a low-odor flame-retardant rubber floor and its preparation method, which improves the generation of low-molecular-weight volatile substances due to aging of the rubber floor due to ultraviolet radiation and oxidation reaction during use by rationally configuring light stabilizers and antioxidants, thus greatly reducing the generation of odor. However, rubber itself has an odor, and additives such as antioxidants also emit a certain odor.
[0004] Thermoplastic elastomer (TPE) is widely used in many technical fields due to its good mechanical properties, recyclability and simple processing methods. Replacing rubber with TPE can effectively solve the problem of odor emitted by rubber itself, but the odor emitted by additives cannot be solved. A TPE odor-free floor and its production process are needed to solve the problem of harmful gases emitted from TPE elastic floors. Summary of the invention
[0005] The purpose of the present invention is to provide a TPE odor-free assembled floor and a production process thereof, so as to solve the problem of how to reduce the emission of harmful gases from the TPE elastic floor.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A TPE odor-free assembled floor, comprising the following raw materials in parts by mass:
[0008] 70-90 parts of composite resin, 10-15 parts of polyvinyl chloride, 40-65 parts of styrene-butadiene-styrene, 4-8 parts of lubricant, 2-6 parts of antioxidant, 10-30 parts of inorganic filler, 5-15 parts of flame retardant, and 4-8 parts of antibacterial agent.
[0009] Further, the composite resin is prepared by the following steps:
[0010] In a reaction kettle, the sulfonic acid porous filler is ultrasonically dispersed in n-butanol, and then bisphenol A epoxy resin is added. After stirring evenly, the temperature is raised to 80-85°C and kept warm for 10-12 hours. After cooling, (3-mercaptopropyl)trimethoxysilane and 4-dimethylaminopyridine are added to the reaction kettle, and stirred at room temperature for 4-6 hours to obtain a composite resin.
[0011] Furthermore, the usage ratio of the sulfonic acid porous filler, n-butanol, bisphenol A epoxy resin, (3-mercaptopropyl)trimethoxysilane and 4-dimethylaminopyridine is 20-40 g: 80-100 mL: 100-120 g: 12-18 g: 0.04-0.05 g.
[0012] Further, the sulfonic acid porous filler is prepared by the following steps:
[0013] Zn(NO3)2·4H2O, sodium 2-thioterephthalate, deionized water and 45wt% hydrofluoric acid are mixed in a Teflon-lined stainless steel autoclave, heated at 180-200°C for 20-24h, cooled to room temperature, centrifuged to collect the precipitate, washed with deionized water 3-5 times, and dried in an oven at 80-100°C for 12-14h to obtain a sulfonic acid-based porous material.
[0014] Furthermore, the usage ratio of Zn(NO3)2·4H2O, sodium 2-thioterephthalate, deionized water and 45wt% hydrofluoric acid is 70-90g:160-200g:2-2.5L:18-22g.
[0015] Furthermore, the lubricant is stearic acid; the inorganic filler is montmorillonite; the flame retardant is ammonium polyphosphate flame retardant; the antibacterial agent is HTB-032 type silver-loaded hydroxy zirconium phosphate nano antibacterial agent; and the antioxidant is 4,4-di(phenylisopropyl)diphenylamine.
[0016] A production process of a TPE odor-free assembled floor comprises the following steps:
[0017] Step 1: Add the composite resin and the inorganic filler into a mixer and mix them at a mixing speed of 600-800 r / min and a mixing time of 15-20 min to obtain a mixed filler resin.
[0018] Step 2: Add polyvinyl chloride, styrene-butadiene-styrene, mixed filler resin, lubricant, antioxidant, flame retardant and antibacterial agent into a double-roll mill for refining at a temperature of 90-110°C. After the rubber is refined, it is calendered for 2-3 minutes on a calender to form it. After vulcanization on a vulcanizer, the TPE odor-free assembled floor is obtained.
[0019] Furthermore, the vulcanization temperature is 140-150°C and the vulcanization pressure is 2.5-3kg / cm 2, vulcanization time 15-20min.
[0020] Beneficial effects of the present invention:
[0021] (1) The TPE odor-free assembled floor prepared by the present invention has an odor-free function, which can absorb the gas generated by the floor internally and reduce the odor emitted by the floor. At the same time, it has good wear resistance, antibacterial and flame retardancy, high tensile strength, and can be used in indoor places such as gyms and dance rooms. The assembly installation method does not require glue to fix, which further reduces the emission of harmful gases and is easy to install.
[0022] (2) The present invention adds a porous filler with gas adsorption capability to the TPE material, thereby improving the wear resistance of the TPE material and adsorbing the gas generated inside the TPE material, thereby greatly reducing the amount of gas emitted from the TPE material.
[0023] (3) The present invention improves the dispersibility of the porous filler in the bisphenol A epoxy resin by reacting and grafting the porous filler with the bisphenol A epoxy resin, and then improves the compatibility of the bisphenol A epoxy resin with PVC and SBS by reacting the mercapto group in (3-mercaptopropyl)trimethoxysilane with the epoxy group, thereby improving the dispersibility of the porous filler in the TPE material, so that the wear resistance of the prepared TPE odor-free assembled floor is improved, and the floor has gas adsorption capacity, thereby improving the odor-free ability of the TPE odor-free assembled floor. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1: A production process of a TPE odor-free assembled floor, comprising the following steps:
[0026] Step 1: 70 g Zn(NO3)2·4H2O, 160 g sodium 2-thioterephthalate, 2 L deionized water and 18 g 45 wt% hydrofluoric acid were mixed in a Teflon-lined stainless steel autoclave, heated at 180°C for 20 h, cooled to room temperature, centrifuged to collect the precipitate, washed 3 times with deionized water, and dried in an oven at 80°C for 12 h to obtain a sulfonic acid porous material; 20 g sulfonic acid porous filler was ultrasonically dispersed in 80 mL n-butanol in a reactor, and then 100 g bisphenol A epoxy resin was added, stirred evenly, and then the temperature was raised to 80°C, kept warm for 10 h, and after cooling, 12 g (3-mercaptopropyl) trimethoxysilane and 0.04 g were added to the reactor. 4-dimethylaminopyridine, stirred at room temperature for 4 hours to obtain a composite resin; 70g of the composite resin and 10g of montmorillonite were added into a mixer for mixing at a mixing speed of 600r / min and a mixing time of 15min to obtain a mixed filler resin.
[0027] Step 2: 10g polyvinyl chloride, 40g styrene-butadiene-styrene (SBS), 80g mixed filler resin, 4g stearic acid, 2g 4,4-di(phenylisopropyl)diphenylamine, 5g ammonium polyphosphate flame retardant and 4g silver-loaded hydroxy zirconium phosphate nano antibacterial agent were added to a double-roll mill for refining at a temperature of 180°C. After the rubber was refining was completed, it was calendered for 2 minutes in a calender to form a shape, and then vulcanized in a vulcanizer at 140°C and 2.5kg / cm 2 After vulcanization for 15 minutes, the TPE odor-free assembled floor was obtained.
[0028] Embodiment 2: A production process of a TPE odor-free assembled floor, comprising the following steps:
[0029] Step 1: 80 g Zn(NO3)2·4H2O, 180 g sodium 2-thioterephthalate, 2.25 L deionized water and 20 g 45 wt% hydrofluoric acid were mixed in a Teflon-lined stainless steel autoclave, heated at 190°C for 22 h, cooled to room temperature, centrifuged to collect the precipitate, washed 4 times with deionized water, and dried in an oven at 90°C for 13 h to obtain a sulfonic acid porous material; 30 g sulfonic acid porous filler was ultrasonically dispersed in 90 mL n-butanol in a reactor, and then 110 g bisphenol A epoxy resin was added, stirred evenly, and then the temperature was raised to 82°C, kept warm for 11 h, and after cooling, 16 g (3-mercaptopropyl) trimethoxysilane and 0.04 g were added to the reactor. 4-dimethylaminopyridine, stirred at room temperature for 5 hours to obtain a composite resin; 80g of the composite resin and 20g of montmorillonite were added into a mixer for mixing at a mixing speed of 700r / min and a mixing time of 17min to obtain a mixed filler resin.
[0030] Step 2: 12g polyvinyl chloride, 50g styrene-butadiene-styrene, 100g mixed filler resin, 6g stearic acid, 4g 4,4-di(phenylisopropyl)diphenylamine, 10g ammonium polyphosphate flame retardant and 6g silver-loaded hydroxy zirconium phosphate nano antibacterial agent were added to a double-roll mill for refining at a temperature of 190°C. After the rubber was refining was completed, it was calendered for 2.5 minutes in a calender and then heated in a vulcanizer at 145°C and 2.75kg / cm 2 After vulcanization for 17 minutes, the TPE odor-free assembled floor was obtained.
[0031] Embodiment 3: A production process of a TPE odor-free assembled floor, comprising the following steps:
[0032] Step 1: 90g Zn(NO3)2·4H2O, 200g sodium 2-thioterephthalate, 2.5L deionized water and 22g 45wt% hydrofluoric acid were mixed in a Teflon-lined stainless steel autoclave, heated at 200°C for 24h, cooled to room temperature, centrifuged to collect the precipitate, washed 5 times with deionized water, and dried in an oven at 100°C for 14h to obtain a sulfonic acid porous material; 40g of the sulfonic acid porous filler was ultrasonically dispersed in 100mL of n-butanol in a reactor, and then 120g of bisphenol A epoxy resin was added, stirred evenly, and then the temperature was raised to 85°C, kept warm for 12h, and after cooling, 18g (3-mercaptopropyl) trimethoxysilane and 0.05g of 1-(2-thio)-1-butylene glycol were added to the reactor. 4-dimethylaminopyridine, stirred at room temperature for 6 hours to obtain a composite resin; 90g of the composite resin and 30g of montmorillonite were added into a mixer for mixing at a mixing speed of 800r / min and a mixing time of 20min to obtain a mixed filler resin.
[0033] Step 2: 15g polyvinyl chloride, 65g styrene-butadiene-styrene, 120g mixed filler resin, 8g stearic acid, 6g 4,4-di(phenylisopropyl)diphenylamine, 15g ammonium polyphosphate flame retardant and 8g silver-loaded hydroxy zirconium phosphate nano antibacterial agent were added to a double-roll mill for refining at a temperature of 200°C. After the rubber was refining was completed, it was calendered for 3 minutes in a calender and then heated in a vulcanizer at 150°C and 3kg / cm 2 After vulcanization for 20 minutes, the TPE odor-free assembled floor was obtained.
[0034] A porous filler with a sulfonic acid group is synthesized so that the porous filler can be grafted into a bisphenol A epoxy resin through the reaction of the sulfonic acid group and the phenol group to obtain a composite resin, and then the mixed resin is mixed with (3-mercaptopropyl)trimethoxysilane so that the mercapto group in the (3-mercaptopropyl)trimethoxysilane reacts with the epoxy group to obtain a mixed resin. (3-mercaptopropyl)trimethoxysilane is used as a coupling agent to improve the compatibility between the mixed resin and SBS and PVC, thereby uniformly dispersing the porous filler and the inorganic filler in the mixed resin. The good compatibility and dispersibility of the mixed resin in SBS and PVC are utilized to uniformly disperse the porous filler and the inorganic filler in the TPE material. The porous filler has a good gas absorption capacity and can absorb the gas generated in the TPE, reduce the release of the gas in the TPE material, and achieve the effect of odor removal.
[0035] Comparative Example 1: The difference from Example 1 is that, in step 1, bisphenol A epoxy resin, sulfonic acid porous filler and montmorillonite are added into a mixer for mixing at a mixing speed of 600 r / min and a mixing time of 15 min to obtain a mixed filler resin.
[0036] Comparative Example 2: The difference from Example 1 is that, in step 1, bisphenol A epoxy resin, activated carbon and montmorillonite are added into a mixer for mixing at a mixing speed of 600 r / min and a mixing time of 15 min to obtain a mixed filler resin.
[0037] Comparative Example 3: The difference from Example 1 is that, in step 1, bisphenol A epoxy resin, activated carbon, montmorillonite and (3-mercaptopropyl)trimethoxysilane are added into a mixer and mixed at a mixing speed of 600 r / min and a mixing time of 15 min to obtain a mixed filler resin.
[0038] In Comparative Examples 2 and 3, the amount of activated carbon added was 20 g.
[0039] The activated carbon was 200 mesh activated carbon powder.
[0040] The sources of some chemical reagents in the embodiments and comparative examples are as follows:
[0041] Styrene-butadiene-styrene was purchased from Dongguan Yingxiang Plastic Raw Materials Co., Ltd.
[0042] Bisphenol A epoxy resin was purchased from Shanghai Kaiyin Chemical Co., Ltd.
[0043] (3-Mercaptopropyl)trimethoxysilane was purchased from Shanghai Myrel Biochemical Technology Co., Ltd.
[0044] Sodium 2-thioterephthalate was purchased from Harbin Kemeis Technology Co., Ltd.
[0045] The remaining reagents were commercially available.
[0046] The performance tests were performed on the TPE odor-free assembled floors prepared in Examples 1 to 3 and Comparative Examples 1 to 3. The vertical deformation, elongation at break and tensile strength of the test samples were tested. The flame retardant properties of the test samples were tested according to GB8624 building material combustion performance. The odor level of the test samples was tested according to GB 36246-2018. The results are shown in Table 1:
[0047] Table 1
[0048] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Vertical deformation 0.70mm 0.72mm 0.75mm 0.81mm 0.83mm 0.79mm Elongation at break 133% 134% 134% 125% 122% 127% Tensile Strength 1.39Mpa 1.36Mpa 1.34Mpa 1.27Mpa 1.28Mpa 1.30Mpa Flame retardant properties B1 B1 B1 B1 B1 B1 Odor level Level 1 Level 1 Level 1 Level 2 Level 2 Level 2
[0049] It can be seen from Table 1 that the vertical deformation of the TPE odor-free assembled floor prepared in Examples 1 to 3 is ≤0.8mm, the elongation at break is ≥130%, the tensile strength is ≥1.3Mpa, the flame retardant grade reaches B1, which meets the test requirements, and the odor level is low, the odor level reaches 1, and the prepared TPE odor-free assembled floor has no odor; Comparative Example 1 Due to the poor dispersion of the sulfonic acid porous filler in the bisphenol A epoxy resin, it not only affects the mechanical properties of the TPE odor-free assembled floor, but also fails to exert the gas adsorption capacity, resulting in a high odor level Although activated carbon with gas adsorption capacity was added to Comparative Example 2, it can be seen from the final performance test data that the activated carbon has a poor gas adsorption effect. The reason is that the dispersibility of the activated carbon in the TPE odor-free assembled floor is poor, resulting in decreased mechanical properties and gas adsorption capacity; Although a silane coupling agent was added to Comparative Example 3, since the activated carbon contains fewer functional groups and has a low degree of cross-linking with the silane coupling agent, the dispersibility of the activated carbon in the TPE odor-free assembled floor is not high. Therefore, the mechanical properties and gas adsorption capacity of Comparative Example 3 are lower than those of Examples 1-3.
[0050] The samples of Example 1 to Example 3 were tested for their antibacterial properties according to the ISO 22196 & GB / T31402-2015 test method. The test bacteria were Candida albicans, Escherichia coli, Klebsiella pneumoniae, and Staphylococcus aureus. The test results showed that the antibacterial rates were all greater than 99%, indicating good antibacterial ability.
[0051] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A TPE odorless assembled floor, It is characterized in that The following raw materials are included by mass: 70-90 parts of composite resin, 10-15 parts of polyvinyl chloride, 40-65 parts of styrene-butadiene-styrene, 4-8 parts of lubricant, 2-6 parts of antioxidant, 10-30 parts of inorganic filler, 5-15 parts of flame retardant, 4-8 parts of antibacterial agent; The composite resin is prepared by the following steps: In a reaction kettle, the sulfonic acid porous filler is ultrasonically dispersed in n-butanol, and then bisphenol A epoxy resin is added. After stirring evenly, the temperature is raised to 80-85°C and kept warm for 10-12 hours. After cooling, (3-mercaptopropyl)trimethoxysilane and 4-dimethylaminopyridine are added to the reaction kettle, and stirred at room temperature for 4-6 hours to obtain a composite resin.
2. The TPE odor-free assembled floor according to claim 1, It is characterized in that The usage ratio of the sulfonic acid porous filler, n-butanol, bisphenol A type epoxy resin, (3-mercaptopropyl)trimethoxysilane and 4-dimethylaminopyridine is 20-40g: 80-100mL: 100-120g: 12-18g: 0.04-0.05g.
3. The TPE odor-free assembled floor according to claim 1, It is characterized in that The sulfonic acid porous filler is prepared by the following steps: Will Zn(NO 3 ) 2 ·4H 2 O, sodium 2-thioterephthalate, deionized water and 45wt% hydrofluoric acid are mixed in a Teflon-lined stainless steel autoclave, heated at 180-200°C for 20-24h, cooled to room temperature, centrifuged to collect the precipitate, washed with deionized water 3-5 times, and dried in an oven at 80-100°C for 12-14h to obtain a sulfonic acid porous material.
4. The TPE odor-free assembled floor according to claim 3, It is characterized in that The Zn(NO 3 ) 2 ·4H 2 The usage ratio of O, sodium 2-thioterephthalate, deionized water and 45wt% hydrofluoric acid is 70-90g:160-200g:2-2.5L:18-22g.
5. The TPE odor-free assembled floor according to claim 1, It is characterized in that The lubricant is stearic acid; the inorganic filler is montmorillonite; the flame retardant is ammonium polyphosphate flame retardant; the antibacterial agent is HTB-032 type silver-loaded hydroxy zirconium phosphate nano antibacterial agent; and the antioxidant is 4,4-di(phenylisopropyl)diphenylamine.
6. The production process of a TPE odor-free assembled floor according to claim 1, It is characterized in that The steps include: Step 1: Add the composite resin and the inorganic filler into a mixer and mix them at a mixing speed of 600-800 r / min for 15-20 min to obtain a mixed filler resin; Step 2: Add polyvinyl chloride, styrene-butadiene-styrene, mixed filler resin, lubricant, antioxidant, flame retardant and antibacterial agent into a double-roll mill for refining at a temperature of 90-110°C. After the rubber is refined, it is calendered for 2-3 minutes on a calender to form it. After vulcanization on a vulcanizer, the TPE odor-free assembled floor is obtained.
7. The production process of the TPE odor-free assembled floor according to claim 6, It is characterized in that The vulcanization temperature is 140-150°C, and the vulcanization pressure is 2.5-3kg / cm 2 , vulcanization time 15-20min.