High-transparency polyester material and preparation method thereof
By adding specific ratios of end-hydroxy hyperbranched polycarbonate and other components to the PET material, combined with the twin-screw extrusion molding process, the problem of insufficient mechanical and aging resistance of PET materials is solved, and high transparency and good quality are achieved Highly transparent polyester material with flame retardancy and long service life is suitable for a wide range of applications.
Patent Information
- Application Number
- CN202411196899.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The mechanical and mechanical properties, aging resistance and impact resistance of existing PET materials are insufficient, and their transparency and flame retardancy need to be further improved, which limits its wide application in the fields of electronics and electrical industries.
PET resin is used as the substrate, combined with terminal hydroxyl hyperbranched polycarbonate, 2-acrylamide-2-methylpropanesulfonic acid, 1,1'-(6,7-dimethyl-2,3-dihydrogen Quinoxaline-1,4-diyl)dipropyl-2-ene-1-one, 2,6-diaminopurine, phosphorus pentoxide, polyphosphoric acid, antioxidant, lubricant, coupling agent, phase The ratio of the container, initiator and filler is made of high-transparent polyester material through a twin-screw extruder molding.
It significantly improves the mechanical and mechanical properties of the material, UV aging resistance and flame retardant properties, maintains high transparency, extends service life, and simplifies the preparation process, which is suitable for continuous large-scale production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester materials, and in particular to a highly transparent polyester material and a preparation method thereof. Background Art
[0002] Thermoplastic polyester materials such as polyethylene terephthalate (PET) have low specific gravity, high strength, high rigidity, good heat resistance, air tightness and toughness, as well as excellent dimensional stability and chemical insulation properties, and are widely used in electronic and electrical components, packaging, automotive industry, etc. However, the mechanical properties, aging resistance and impact resistance of pure PET materials are not enough, which limits its wider application.
[0003] In order to improve the physical properties of PET materials, the conventional method is to add functional fillers or additives; however, the addition of a large amount of functional fillers or additives will affect the processing fluidity and comprehensive performance of the product; due to compatibility issues, these functional additives or fillers are easy to leak out from the inside of the material, affecting the product appearance and performance stability. In addition, these methods will also affect the transparency of PET materials, reduce its optical properties, and in turn limit its application in the optical field.
[0004] For example, the Chinese invention patent with the authorization announcement number CN113980436B discloses a modified polyester transparent composite material and its preparation method. The composite material described in the invention is made of resin materials through blending and molding processes. The resin materials include the following components by mass: 60 to 80 parts of polyester resin; 15 to 28 parts of methyl methacrylate polymer; 5 to 12 parts of compatibilizer; the polyester resin is a thermoplastic aromatic polyester; the compatibilizer is an acrylic polyol monoester. The modified polyester transparent composite material provided by the invention has high light transmittance, extremely low haze, good physical and mechanical strength and toughness, and good scratch resistance. It can be widely used in various types of food, medicine, non-toxic and sterile packaging materials, textiles, precision instruments, high-end packaging materials for electronic components, and transparent shells for automotive accessories and electronic appliances. However, the UV aging resistance and flame retardancy of the material still need to be further improved.
[0005] Therefore, the development of a highly transparent polyester material with good mechanical properties, excellent UV aging resistance and flame retardant properties, sufficient transparency and long service life and its preparation method meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the polyester material field. Summary of the invention
[0006] In view of the above problems, the object of the present invention is to provide a highly transparent polyester material with good mechanical properties, excellent UV aging resistance and flame retardant properties, sufficient transparency and long service life, and a preparation method thereof.
[0007] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a highly transparent polyester material, comprising the following raw materials in parts by weight: 80 parts of PET resin, 15-25 parts of terminal hydroxyl hyperbranched polycarbonate, 4-8 parts of 2-acrylamide-2-methylpropane sulfonic acid, 3-5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 1-3 parts of 2,6-diaminopurine, 0.5-0.8 parts of phosphorus pentoxide, 0.3-0.5 parts of polyphosphoric acid, 0.8-1.2 parts of antioxidant, 0.6-0.8 parts of lubricant, 1-3 parts of coupling agent, 1-2 parts of compatibilizer, 0.8-1.2 parts of initiator, and 10-20 parts of filler.
[0008] Preferably, the PET resin is at least one of DSR TL-103 PET resin produced by Xiamen Tenglong, China, PET008L resin produced by Aclo Compounders, Canada, and YS-W01 PET resin produced by Hainan Yisheng Petrochemical, China.
[0009] Preferably, there is no special requirement for the source of the terminal hydroxyl hyperbranched polycarbonate. In one embodiment of the present invention, the terminal hydroxyl hyperbranched polycarbonate is prepared according to the method of Example 5 of Chinese invention patent with authorization announcement number CN107151316B.
[0010] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168; and the lubricant is selected from any one or more of polyethylene wax, oxidized polyethylene wax, or paraffin wax.
[0011] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the compatibilizer is at least one of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH, and PP-g-MAH.
[0012] Preferably, the initiator is at least one of methyl ethyl ketone peroxide, cyclohexanone peroxide, and diisopropylbenzene peroxide.
[0013] Preferably, the filler is a transparent powder with a particle size of 550-1250 mesh.
[0014] Another object of the present invention is to provide a method for preparing the highly transparent polyester material, comprising the following steps: uniformly mixing the raw materials by weight to obtain a mixture, and then adding the mixture to a twin-screw extruder for extrusion molding to obtain a highly transparent polyester material.
[0015] Preferably, the extrusion temperature of the twin-screw extruder is 235-255° C., and the screw speed is 230-330 r / min.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The preparation method of the highly transparent polyester material disclosed in the present invention has simple process, convenient operation and control, high preparation efficiency and finished product qualification rate, low dependence on equipment, low energy consumption, suitable for continuous large-scale production, and high promotion and application value.
[0018] (2) The highly transparent polyester material disclosed in the present invention is made of the following raw materials in parts by weight: 80 parts of PET resin, 15-25 parts of terminal hydroxyl hyperbranched polycarbonate, 4-8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 3-5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 1-3 parts of 2,6-diaminopurine, 0.5-0.8 parts of phosphorus pentoxide, 0.3-0.5 parts of polyphosphoric acid, 0.8-1.2 parts of antioxidant, 0.6-0.8 parts of lubricant, 1-3 parts of coupling agent, 1-2 parts of compatibilizer, 0.8-1.2 parts of initiator, and 10-20 parts of filler. Through the mutual cooperation between the raw materials, the polyester material product has good mechanical properties, excellent UV aging resistance and flame retardancy, sufficient transparency, and long service life.
[0019] (3) The highly transparent polyester material disclosed in the present invention uses PET resin and terminal hydroxyl hyperbranched polycarbonate as the base material, combining the advantages of the two, and improving the toughness of the material under the premise of ensuring the high transparency of the material; through the reasonable selection of other raw material types and their dosage ratios, hyperbranched polycarbonate structure, polyester structure, quinoxalinone structure, and purine structure are simultaneously introduced into the molecular structure of the material. Under the multiple effects of these structures such as electronic effect, steric effect, and conjugation effect, the mechanical properties of the manufactured product are better, the UV aging resistance and flame retardancy are better, the transparency is sufficient, and the service life is longer. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.
[0021] Example 1
[0022] A highly transparent polyester material comprises the following raw materials in parts by weight: 80 parts of PET resin, 15 parts of terminal hydroxyl hyperbranched polycarbonate, 4 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 1 part of 2,6-diaminopurine, 0.5 parts of phosphorus pentoxide, 0.3 parts of polyphosphoric acid, 0.8 parts of antioxidant, 0.6 parts of lubricant, 1 part of coupling agent, 1 part of compatibilizer, 0.8 parts of initiator and 10 parts of filler.
[0023] The PET resin is Tenglong DSR TL-103PET resin from Xiamen, China; the terminal hydroxyl hyperbranched polycarbonate is made according to the method of Example 5 of the Chinese invention patent with authorization announcement number CN107151316B; the antioxidant is antioxidant 1010; the lubricant is selected from polyethylene wax; the coupling agent is silane coupling agent KH550; the compatibilizer is PE-g-ST; the initiator is methyl ethyl ketone peroxide; the filler is transparent powder with a particle size of 550 mesh.
[0024] A preparation method of the highly transparent polyester material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain the highly transparent polyester material; the extrusion temperature of the twin-screw extruder is 235°C and the screw speed is 230r / min.
[0025] Example 2
[0026] A highly transparent polyester material comprises the following raw materials in parts by weight: 80 parts of PET resin, 18 parts of terminal hydroxyl hyperbranched polycarbonate, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3.5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 1.5 parts of 2,6-diaminopurine, 0.6 parts of phosphorus pentoxide, 0.35 parts of polyphosphoric acid, 0.9 parts of antioxidant, 0.65 parts of lubricant, 1.5 parts of coupling agent, 1.2 parts of compatibilizer, 0.9 parts of initiator and 13 parts of filler.
[0027] The PET resin is Tenglong DSR TL-103PET resin from Xiamen, China; the terminal hydroxyl hyperbranched polycarbonate is prepared according to the method of Example 5 of the Chinese invention patent with authorization announcement number CN107151316B; the antioxidant is antioxidant 1076; the lubricant is oxidized polyethylene wax; the coupling agent is silane coupling agent KH560; the compatibilizer is PP-g-ST; the initiator is cyclohexanone peroxide; the filler is transparent powder with a particle size of 800 mesh.
[0028] A preparation method of the highly transparent polyester material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain the highly transparent polyester material; the extrusion temperature of the twin-screw extruder is 240°C and the screw speed is 250r / min.
[0029] Example 3
[0030] A highly transparent polyester material comprises the following raw materials in parts by weight: 80 parts of PET resin, 20 parts of terminal hydroxyl hyperbranched polycarbonate, 6 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 2 parts of 2,6-diaminopurine, 0.65 parts of phosphorus pentoxide, 0.4 parts of polyphosphoric acid, 1 part of antioxidant, 0.7 parts of lubricant, 2 parts of coupling agent, 1.5 parts of compatibilizer, 1 part of initiator and 15 parts of filler.
[0031] The PET resin is Tenglong DSR TL-103PET resin from Xiamen, China; the terminal hydroxyl hyperbranched polycarbonate is prepared according to the method of Example 5 of the Chinese invention patent with authorization announcement number CN107151316B; the antioxidant is antioxidant 168; the lubricant is paraffin; the coupling agent is silane coupling agent KH570; the compatibilizer is ABS-g-MAH; the initiator is diisopropylbenzene peroxide; the filler is transparent powder with a particle size of 900 mesh.
[0032] A preparation method of the highly transparent polyester material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain the highly transparent polyester material; the extrusion temperature of the twin-screw extruder is 245°C and the screw speed is 290r / min.
[0033] Example 4
[0034] A highly transparent polyester material is made of the following raw materials in parts by weight: 80 parts of PET resin, 23 parts of terminal hydroxyl hyperbranched polycarbonate, 7 parts of 2-acrylamide-2-methylpropanesulfonic acid, 4.5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 2.5 parts of 2,6-diaminopurine, 0.75 parts of phosphorus pentoxide, 0.45 parts of polyphosphoric acid, 1.1 parts of antioxidant, 0.75 parts of lubricant, 2.5 parts of coupling agent, 1.8 parts of compatibilizer, 1.1 parts of initiator and 18 parts of filler.
[0035] The PET resin is DSR TL-103PET resin from Xiamen Tenglong, China; the terminal hydroxyl hyperbranched polycarbonate is prepared according to the method of Example 5 of the Chinese invention patent with the authorization announcement number CN107151316B; the antioxidant is a mixture of antioxidant 1010, antioxidant 1076, and antioxidant 168 in a mass ratio of 1:2:3; the lubricant is a mixture of polyethylene wax, oxidized polyethylene wax, and paraffin in a mass ratio of 1:1:2; the coupling agent is a silane coupling agent KH550, A mixture formed by mixing silane coupling agent KH560 and silane coupling agent KH570 in a mass ratio of 1:1:1; the compatibilizer is a mixture of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH, and PP-g-MAH in a mass ratio of 1:2:3:2:1; the initiator is a mixture of methyl ethyl ketone peroxide, cyclohexanone peroxide, and diisopropylbenzene peroxide in a mass ratio of 1:3:5; the filler is a transparent powder with a particle size of 1200 mesh.
[0036] A preparation method of the highly transparent polyester material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain the highly transparent polyester material; the extrusion temperature of the twin-screw extruder is 250°C and the screw speed is 320r / min.
[0037] Example 5
[0038] A highly transparent polyester material comprises the following raw materials in parts by weight: 80 parts of PET resin, 25 parts of terminal hydroxyl hyperbranched polycarbonate, 8 parts of 2-acrylamido-2-methylpropanesulfonic acid, 5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 3 parts of 2,6-diaminopurine, 0.8 parts of phosphorus pentoxide, 0.5 parts of polyphosphoric acid, 1.2 parts of antioxidant, 0.8 parts of lubricant, 3 parts of coupling agent, 2 parts of compatibilizer, 1.2 parts of initiator and 20 parts of filler.
[0039] The PET resin is Tenglong DSR TL-103PET resin from Xiamen, China; the terminal hydroxyl hyperbranched polycarbonate is made according to the method of Example 5 of the Chinese invention patent with authorization announcement number CN107151316B; the antioxidant is antioxidant 1010; the lubricant is polyethylene wax; the coupling agent is silane coupling agent KH550; the compatibilizer is PP-g-MAH; the initiator is cyclohexanone peroxide; the filler is transparent powder with a particle size of 1250 mesh.
[0040] A preparation method of the highly transparent polyester material comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain the highly transparent polyester material; the extrusion temperature of the twin-screw extruder is 255°C and the screw speed is 330r / min.
[0041] Comparative Example 1
[0042] A highly transparent polyester material is substantially the same as Example 1, except that 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)bisprop-2-en-1-one is not added.
[0043] Comparative Example 2
[0044] A highly transparent polyester material is substantially the same as Example 1, except that 2,6-diaminopurine is not added.
[0045] In order to further illustrate the unexpected positive technical effects achieved by the products of each embodiment of the present invention, the high-transparent polyester materials prepared in each example were tested for relevant properties. The test results are shown in Table 1. The test method is as follows:
[0046] (1) Tensile properties: The tensile strength is tested according to GB / T 1040.1-2018.
[0047] (2) UV aging resistance: Each polyester material sample was irradiated with UV light of 350 nm wavelength at room temperature for 48 hours, with the sample 10 cm away from the UV light source. The UV aging resistance was measured by the retention rate of tensile strength. The larger the value, the better the UV aging resistance.
[0048] (3) Flame retardancy: tested according to UL-94.
[0049] (4) Impact performance: The impact performance of the specimens was tested using an Izod notch impact tester in accordance with ASTM D256-2018 Standard Test Methods for Determining the Izod Pendulum Impact Resistance of Plastics. The specimen type was Type II, Type A notch, the specimen thickness was 3.2 mm ± 0.2 mm, and the test temperature was 23 °C ± 0.5 °C.
[0050] (5) Light transmittance: A spectrophotometer was used to measure the light transmittance of a sample strip at a wavelength of 550 nm with reference to ASTM D1003-2013 Light transmittance and haze of transparent plastics. The thickness of the sample strip was 3.0 mm.
[0051] Table 1
[0052] project Tensile Strength Flame retardant UV aging resistance Impact strength Light transmittance unit MPa class % J / m % Example 1 78 V-0 99.35 46 90 Example 2 80 V-0 99.46 48 90 Example 3 83 V-0 99.61 51 91 Example 4 88 V-0 99.82 52 92 Example 5 90 V-0 99.95 54 92 Comparative Example 1 72 V-1 98.73 43 89 Comparative Example 2 69 V-2 98.19 41 88
[0053] It can be seen from Table 1 that the high-transparency polyester material disclosed in the embodiment of the present invention has better mechanical properties, flame retardancy, UV aging resistance and impact toughness than the comparative example product, and has high transparency. The addition of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)bisprop-2-en-1-one and 2,6-diaminopurine is beneficial to improving the above properties.
[0054] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as described above. However, any technician familiar with the profession can make some changes, modifications and evolutions of the technical content disclosed above without departing from the scope of the technical solution of the present invention, which are all equivalent embodiments of the present invention. At the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A highly transparent polyester material, characterized in that: The invention comprises the following raw materials in parts by weight: 80 parts of PET resin, 15-25 parts of terminal hydroxyl hyperbranched polycarbonate, 4-8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 3-5 parts of 1,1'-(6,7-dimethyl-2,3-dihydroquinoxaline-1,4-diyl)diprop-2-ene-1-one, 1-3 parts of 2,6-diaminopurine, 0.5-0.8 parts of phosphorus pentoxide, 0.3-0.5 parts of polyphosphoric acid, 0.8-1.2 parts of antioxidant, 0.6-0.8 parts of lubricant, 1-3 parts of coupling agent, 1-2 parts of compatibilizer, 0.8-1.2 parts of initiator and 10-20 parts of filler.
2. The highly transparent polyester material according to claim 1, characterized in that: The PET resin is at least one of the following: DSRTL-103 PET resin produced by Xiamen Tenglong, China, PET008L resin produced by Aclo Compounders, Canada, and YS-W01 PET resin produced by Hainan Yisheng Petrochemical, China.
3. The highly transparent polyester material according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168; the lubricant is selected from any one or more of polyethylene wax, oxidized polyethylene wax, or paraffin wax.
4. The highly transparent polyester material according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the compatibilizer is at least one of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH, and PP-g-MAH.
5. The highly transparent polyester material according to claim 1, characterized in that: The initiator is at least one of methyl ethyl ketone peroxide, cyclohexanone peroxide and dicumyl peroxide.
6. The highly transparent polyester material according to claim 1, characterized in that: The filler is transparent powder with a particle size of 550-1250 meshes.
7. A method for preparing the highly transparent polyester material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: uniformly mixing the raw materials according to weight to obtain a mixture, and then adding the mixture into a twin-screw extruder for extrusion molding to obtain a highly transparent polyester material.
8. The method for preparing the highly transparent polyester material according to claim 7, characterized in that: The extrusion temperature of the twin-screw extruder is 235-255° C., and the screw speed is 230-330 r / min.
Citation Information
Patent Citations
High-strength high-toughness flame-retardant polypropylene composite material and preparation method thereof
CN114085458A
Heat-resistant environment-friendly cable material and preparation method thereof
CN114350098A
Environment-friendly polypropylene composite material and preparation method thereof
CN114621526A
High-strength anti-aging polymer composite material and preparation method thereof
CN117820848A
High-toughness biaxially oriented nylon film and production method thereof
CN120209561A
Cited By
Impact-resistant high-toughness plastic as well as preparation method and application thereof
CN119639207A
Reinforced flame-retardant PC composite material and preparation method thereof
CN120737576A