Silica gel self-leveling insulation plugging material and preparation method thereof
Through the silicone self-leveling insulating sealing material, combined with the reaction of vinyl silicone oil and Kathan PT catalyst, a material with fire-resistant, flame-retardant, electrical insulation and water-resistant properties is formed, solving the problem of the existing technology in humid, high voltage and low temperature environments. The reliability issue has achieved the goal of convenient construction and cost-effectiveness.
Patent Information
- Application Number
- CN202410882406.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-26
AI Technical Summary
The existing cabinet cable sealing materials are difficult to ensure reliability in humid, high voltage and low temperature environments, and the construction process requires simple and no damage to the cables. The material price cannot be too high, and lacks low temperature resistance, fire resistance, moisture resistance and insulation performance. Good material.
Silicone self-leveling insulation sealing materials are used, including material A and material B. Material A is composed of vinyl silicone oil, hydrogen-containing silicone oil, nano-silica, expanded graphite and aluminum hydroxide. Material B is composed of vinyl silicone oil and nano-dioxide. Silicon and Kathleen PT catalysts are composed of which adjust the curing time by adjusting the catalyst ratio to form materials with fire-resistant, flame-retardant, electrical insulation and waterproof properties.
It provides a sealing material with good low temperature resistance, fire resistance, moisture resistance and insulation performance, which is convenient to construct, suitable for humid and high voltage environments, and can adjust the curing time according to on-site demand to ensure the stable performance of the material below -40℃.
Smart Images

Figure CN119019849A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plugging materials, and in particular to a silica gel self-leveling insulating plugging material and a preparation method thereof. Background Art
[0002] There are two main types of existing cabinet cable sealing: 1) fireproof mud, fireproof sandbags, and modular sealing, all of which are local sealing, and 2) self-leveling materials; currently, both materials are intended to solve room temperature fire protection.
[0003] In fact, cabinet plugging is mostly used in humid, high-voltage, and dirty environments. For example, the ring network cabinets on the roadside in the city, the outdoor cabinets of the hydropower station, the outdoor signal station of the telecommunications company, etc., are often exposed to cold environments such as rain, snow, and ice. The groundwater level in the south is very high, humid, and flooded; the winter in the north is as cold as -30 to -40 degrees. The construction of cable plugging also needs to be simple, and the laid cables cannot be damaged during the construction process. The material price cannot be too expensive, and the reliability of cable and pipeline plugging must be guaranteed. Therefore, there is an urgent need for a plugging material that is resistant to low temperatures, fireproof, moisture-proof, has good insulation properties, and is easy to construct. Summary of the invention
[0004] In order to solve the problems in the prior art, the present invention provides a silica gel self-leveling insulation plugging material and a preparation method thereof.
[0005] On the one hand, a silicone self-leveling insulation plugging material is provided, comprising: material A and material B;
[0006] The material A comprises: 100 parts of vinyl silicone oil, 1-8 parts of hydrogen-containing silicone oil, 1-5 parts of nano silicon dioxide, 8-15 parts of expanded graphite and 5-10 parts of aluminum hydroxide;
[0007] The second material comprises: 100 parts of vinyl silicone oil, 1-5 parts of nano silicon dioxide and 0.5-3 parts of Karl Fischer-Tropsch catalyst.
[0008] Furthermore, the weight ratio of the material A to the material B is 5:1.
[0009] Furthermore, the curing time of the silicone self-leveling insulating sealing material is 5 minutes to 24 hours.
[0010] On the other hand, a method for preparing the silicone self-leveling insulating sealing material is provided, comprising:
[0011] Mix 100 parts of vinyl silicone oil, 1 to 8 parts of hydrogen-containing silicone oil, 1 to 5 parts of nano-silicon dioxide, 8 to 15 parts of expanded graphite and 5 to 10 parts of aluminum hydroxide to obtain material A;
[0012] Mix 100 parts of vinyl silicone oil, 1 to 5 parts of nano-silicon dioxide and 0.5 to 3 parts of Karl Fischer-Tropsch catalyst to obtain material B;
[0013] The material B is poured into the material A and stirred to obtain the silica gel self-leveling insulating sealing material.
[0014] Furthermore, the final stirring time after mixing material A and material B is 1 to 2 minutes.
[0015] Furthermore, the curing time of the silicone self-leveling insulating sealing material is adjusted to 5 minutes to 24 hours by adjusting the ratio between the vinyl silicone oil and the Castor PT catalyst in the second material.
[0016] The technical solution provided by the embodiment of the present invention has the following beneficial effects: the present invention includes material A and material B, material A includes: 100 parts of vinyl silicone oil, 1-8 parts of hydrogen-containing silicone oil, 1-5 parts of nano-silicon dioxide, 8-15 parts of expanded graphite and 5-10 parts of aluminum hydroxide; material B includes: 100 parts of vinyl silicone oil, 1-5 parts of nano-silicon dioxide and 0.5-3 parts of Caterpillar PT catalyst. After material A and material B are mixed, under the action of the Caterpillar PT catalyst of material B, the vinyl silicone oil and hydrogen-containing silicone oil in material A and material B react and combine into macromolecules to obtain a silicone self-leveling insulating sealing material with fireproof, flame retardant, electrical insulating and waterproof properties.
[0017] Secondly, the silicone self-leveling insulation sealing material is divided into material A and material B before use to facilitate long-term storage and transportation.
[0018] In addition, due to different on-site environments, the required curing time of the sealing material will also be different. Therefore, the curing time of the silicone self-leveling insulating sealing material can be adjusted by adjusting the ratio between the vinyl silicone oil and the CAT catalyst in the second material. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 The present invention provides a flow chart of a method for preparing a silicone self-leveling insulating plugging material. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0022] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0023] Embodiment 1
[0024] A silicone self-leveling insulating sealing material comprises: material A and material B; wherein material A comprises: 100 parts of vinyl silicone oil, 1 part of hydrogenated silicone oil, 1 part of nano-silicon dioxide, 8 parts of expanded graphite and 5 parts of aluminum hydroxide; material B comprises: 100 parts of vinyl silicone oil, 1 part of nano-silicon dioxide and 0.5 part of Cationic PT catalyst; the weight ratio of material A to material B is 5:1.
[0025] The preparation method of the silicone self-leveling insulating plugging material comprises: mixing 100 parts of vinyl silicone oil, 1 part of hydrogenated silicone oil, 1 part of nano-silicon dioxide, 8 parts of expanded graphite and 5 parts of aluminum hydroxide to obtain material A; mixing 100 parts of vinyl silicone oil, 1 part of nano-silicon dioxide and 0.5 parts of Catelyn PT catalyst to obtain material B; when it is needed, pouring material B into material A and stirring for 1 minute with a hand drill and a stirrer to obtain the silicone self-leveling insulating plugging material, pouring the silicone self-leveling insulating plugging material into a position to be blocked, and curing after 24 hours.
[0026] Embodiment 2
[0027] A silicone self-leveling insulating sealing material comprises: material A and material B; wherein material A comprises: 100 parts of vinyl silicone oil, 4 parts of hydrogenated silicone oil, 2 parts of nano silicon dioxide, 11 parts of expanded graphite and 7 parts of aluminum hydroxide; material B comprises: 100 parts of vinyl silicone oil, 3 parts of nano silicon dioxide and 1.5 parts of Cationic PT catalyst; the weight ratio of material A to material B is 5:1.
[0028] The preparation method of the silicone self-leveling insulating plugging material comprises: mixing 100 parts of vinyl silicone oil, 4 parts of hydrogenated silicone oil, 2 parts of nano-silicon dioxide, 11 parts of expanded graphite and 7 parts of aluminum hydroxide to obtain material A; mixing 100 parts of vinyl silicone oil, 3 parts of nano-silicon dioxide and 1.5 parts of Catelyn PT catalyst to obtain material B; when it is needed, pouring material B into material A and stirring it for 2 minutes with a hand drill and a stirrer to obtain the silicone self-leveling insulating plugging material, and pouring the silicone self-leveling insulating plugging material into a position to be plugged and solidifying it after 10 hours.
[0029] Embodiment 3
[0030] A silicone self-leveling insulating plugging material comprises: material A and material B; wherein material A comprises: 100 parts of vinyl silicone oil, 8 parts of hydrogenated silicone oil, 5 parts of nano silicon dioxide, 15 parts of expanded graphite and 10 parts of aluminum hydroxide; material B comprises: 100 parts of vinyl silicone oil, 5 parts of nano silicon dioxide and 3 parts of Cationic PT catalyst; the weight ratio of material A to material B is 5:1.
[0031] The preparation method of the silicone self-leveling insulating plugging material comprises: mixing 100 parts of vinyl silicone oil, 8 parts of hydrogenated silicone oil, 5 parts of nano-silicon dioxide, 15 parts of expanded graphite and 10 parts of aluminum hydroxide to obtain material A; mixing 100 parts of vinyl silicone oil, 5 parts of nano-silicon dioxide and 3 parts of Cathol PT catalyst to obtain material B; when it is needed, pouring material B into material A and stirring for 2 minutes with a hand drill with a stirrer to obtain the silicone self-leveling insulating plugging material, and pouring the silicone self-leveling insulating plugging material into a position to be blocked, and solidifying after 5 minutes.
[0032] It should be noted that, firstly, in the silicone self-leveling insulating sealing material, material A is used to provide most of the raw materials for the final mixed reactant, and material B is prepared to make material A (vinyl silicone oil and hydrogen-containing silicone oil) and material A and material B (hydrogen-containing silicone oil in material A and vinyl silicone oil and Carfghan catalyst in material B) react; and the purpose of distinguishing material A from material B before use is for long-term storage and transportation.
[0033] Secondly, due to the different on-site environments, the required curing time of the sealing materials will also be different. For example: if there is a requirement for rapid leak plugging on site, rapid solidification is required, such as a few minutes. If the site requires sufficient construction time, such as in places that are difficult to access, several hours of construction time is required. In this way, the solidification time of the material cannot be too short, such as 12 to 24 hours. Moreover, the room temperature is different in summer and winter, and the solidification time of materials with the same formula is also different. Therefore, the curing time of the silicone self-leveling insulation sealing material can be adjusted by adjusting the ratio between the vinyl silicone oil and the Cas PT catalyst in the second material. The curing time is 5 minutes to 24 hours. The higher the proportion of the Cas PT catalyst in the second material, the shorter the curing time.
[0034] In addition, after material A and material B are mixed, under the action of the Catena PT catalyst in material B, the vinyl silicone oil and hydrogen-containing silicone oil in material A and material B react and combine into macromolecules to obtain the silicone self-leveling insulating sealing material; nano silicon dioxide can improve the mechanical strength of the product, expanded graphite and aluminum hydroxide are flame retardants, and by appropriately adjusting the proportions between the various components, a silicone self-leveling insulating sealing material with fireproof, flame retardant, electrical insulating and waterproof properties can be prepared, and the performance does not change much at a low temperature of -40°C.
[0035] It should also be noted that the silicone self-leveling insulating plugging materials prepared in Example 1, Example 2 and Example 3 were subjected to insulation withstand voltage tests by the Institute of High Voltage Physics and Engineering High Voltage Physics of the Institute of Gas Science and Technology of Xi'an Jiaotong University. The insulation test items were carried out according to the provisions of 5.3 rated insulation level in GB / T 11022-2020 "Common Technical Requirements for High-voltage AC Switchgear and Control Equipment Standards"; the withstand voltage test was to place the test material between two flat electrodes, with the upper electrode applying pressure and the lower electrode grounded. See Table 1 for experimental data.
[0036] Table 1: Insulation withstand voltage test
[0037]
[0038] From the test data in Table 1, we can see that the three samples provided have passed the 50kV, 1 minute power frequency withstand voltage test and the 95kV standard lightning impulse test, 15 times each for positive and negative polarity, without discharge. The results show that the sample has passed the insulation withstand test. Among them, the test room temperature: 18.5℃; relative humidity 64%; air pressure: 98.07kpa, the test sample size is 300*300*15mm.
[0039] In addition, the vertical combustion and oxygen index tests of the silicone self-leveling insulating sealing material in Example 2 of the present invention were carried out by the National Fireproof Building Materials Quality Inspection and Testing Center (NFTC) of the Sichuan Fire Research Institute (SCFRI) of the Ministry of Emergency Management. The inspection was based on GB / T 2408-2021 "Horizontal and vertical methods for determination of combustion performance of plastics"; GB / T 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test", and the test data can be found in Table 2.
[0040] Table 2: Vertical combustion performance, oxygen index
[0041]
[0042]
[0043] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A silicone self-leveling insulation plugging material, It is characterized in that include: Material A and Material B; The material A comprises: 100 parts of vinyl silicone oil, 1-8 parts of hydrogen-containing silicone oil, 1-5 parts of nano silicon dioxide, 8-15 parts of expanded graphite and 5-10 parts of aluminum hydroxide; The second material comprises: 100 parts of vinyl silicone oil, 1-5 parts of nano silicon dioxide and 0.5-3 parts of Karl Fischer-Tropsch catalyst.
2. The silicone self-leveling insulating plugging material according to claim 1, It is characterized in that The weight ratio of the material A to the material B is 5:
1.
3. The silica gel self-leveling insulating plugging material according to claim 1, It is characterized in that The curing time of the silica gel self-leveling insulating sealing material is 5 minutes to 24 hours.
4. A method for preparing the silicone self-leveling insulating plugging material according to any one of claims 1 to 3, It is characterized in that include: Mix 100 parts of vinyl silicone oil, 1 to 8 parts of hydrogen-containing silicone oil, 1 to 5 parts of nano-silicon dioxide, 8 to 15 parts of expanded graphite and 5 to 10 parts of aluminum hydroxide to obtain material A; Mix 100 parts of vinyl silicone oil, 1 to 5 parts of nano-silicon dioxide and 0.5 to 3 parts of Karl Fischer-Tropsch catalyst to obtain material B; The material B is poured into the material A and stirred to obtain the silica gel self-leveling insulating sealing material.
5. The method for preparing the silica gel self-leveling insulating plugging material according to claim 4, It is characterized in that The final stirring time after mixing material A and material B is 1 to 2 minutes.
6. The method for preparing the silica gel self-leveling insulating plugging material according to claim 4, It is characterized in that The curing time of the silicone self-leveling insulating sealing material is adjusted to 5 minutes to 24 hours by adjusting the ratio between the vinyl silicone oil and the Castor PT catalyst in the second material.