Fireproof and heat-insulating coating applicable to 500-800 DEG C as well as preparation method and application of fireproof and heat-insulating coating

By optimizing the ratio of binders and fibers, the ablation resistance and cracking resistance of fire-resistant thermal insulation coatings of 500℃-800℃ are improved, and the problem of poor thermal insulation effect of existing fire-resistant coatings at high temperatures is solved, satisfying the problem of Fire protection requirements for high-rise/super-high-rise buildings.

CN119019871APending Publication Date: 2024-11-26SICHUAN FIRE RES INST OF MEM
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411090037.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing non-expanded fire-resistant coatings suitable for 500℃-800℃ have low ablation resistance, crack resistance and fire resistance, making it difficult to meet the fire protection needs of high-rise/super-high-rise buildings.

Method used

Use black silicate binder, white silicate binder, expanded perlite, expanded vermiculite, mica, hydroxypropyl cellulose, ethylene vinyl acetate emulsion, sodium dodecyl sulfate, film forming additives , raw materials such as zirconium aluminum silicate fiber and alumina fiber, improve the strength and crack resistance of fire-resistant and heat-resistant coatings by optimizing the ratio of binders and fibers, and reduce smoke production and toxicity.

Benefits of technology

It improves the ablation resistance, cracking resistance and fire resistance of fire insulation coatings, enhances its thermal insulation effect at high temperatures, and reduces the fire risk of high-rise/super-high-rise buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019871A_ABST
    Figure CN119019871A_ABST
Patent Text Reader

Abstract

The invention discloses a fireproof heat-insulating coating applicable to 500-800 DEG C as well as a preparation method and an application of the fireproof heat-insulating coating. The fireproof heat-insulating coating applicable to the temperature of 500-800 DEG C is prepared from a black silicate binder, a white silicate binder, expanded perlite, expanded vermiculite, floating beads, mica, hydroxy propyl cellulose, ethylene vinyl acetate emulsion, lauryl sodium sulfate, a coalescing agent TX12, zirconium-containing aluminum silicate fibers, 1, 2-propylene glycol, alumina fibers and water. The invention also discloses an application of the fireproof heat-insulating coating in preparation of a fireproof heat-insulating layer suitable for 500-800 DEG C. The fireproof heat-insulating layer is obtained by paving the fireproof heat-insulating coating on a steel plate and naturally curing the fireproof heat-insulating coating. The fireproof heat-insulating coating suitable for 500-800 DEG C has good ablation resistance, cracking resistance and fireproof strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fireproof materials, and in particular to a fireproof and heat-insulating coating suitable for 500-800°C, a preparation method and application thereof. Background Art

[0002] In recent years, fire accidents in high-rise / super-high-rise buildings have occurred frequently, and high-rise / building fires have a fast vertical spread speed, a large number of combustibles, difficulty in external rescue, high risks of smoke and toxic gases, and a lack of major rescue means. High-rise / super-high-rise buildings still rely mainly on self-rescue. Therefore, improving the fire protection level and protection effect of buildings has been mentioned as the primary consideration. According to the fire protection characteristics of high-rise / super-high-rise buildings, facing the requirements of high fire resistance limit, good weather resistance, good flexibility, high strength, easy construction, and low surface density of fire protection materials, it is urgent to develop fireproof materials that meet the characteristics of high-rise / super-high-rise buildings. Existing fireproof materials have the problems of large unit area weight and low comprehensive cost performance, which makes it difficult to fully adapt to the characteristics of high-rise / super-high-rise buildings. Therefore, it is urgent to optimize the structure of protective materials to adapt to the multi-layer fire protection technology of different temperature sections and different fireproof materials, so as to improve the comprehensive cost performance of fire protection products and adapt them to the characteristics of high-rise / super-high-rise fire protection, so as to provide long-term fire protection for high-rise / super-high-rise buildings.

[0003] Among the existing high-rise fire protection products, fireproof panels and fireproof coatings have the most mature technology, and can meet the fire resistance limit requirements of 3.00h-4.00h for high-rise / super-high-rise walls or load-bearing structures. According to national standard classification, my country's steel structure fire retardant coatings are mainly divided into intumescent steel structure fire retardant coatings and non-intumescent steel structure fire retardant coatings. At present, in the domestic high-rise and super-high-rise steel structure (or fire resistance limit exceeds 2.50h) building fire protection design, it is recommended to use non-intumescent steel structure fire retardant coatings, which are mainly used for fire protection of load-bearing components. Non-intumescent steel structure fire retardant coatings are further divided into non-intumescent fire retardant coatings suitable for different temperature ranges of 500℃-800℃ and 800℃-1200℃, while the existing non-intumescent fire retardant coatings suitable for 500℃-800℃ have low ablation resistance, cracking resistance and fire resistance strength. Summary of the invention

[0004] The purpose of the present invention is to provide a fireproof and heat-insulating coating suitable for 500℃-800℃ and a preparation method thereof, so as to solve the technical problems of low ablation resistance, cracking resistance and fireproof strength of non-expanding fireproof coating suitable for 500℃-800℃.

[0005] Another object of the present invention is to provide an application of the fireproof and heat-insulating coating in the preparation of a fireproof and heat-insulating layer suitable for 500°C-800°C.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] The invention discloses a fireproof and heat-insulating coating suitable for 500-800 DEG C. The coating is prepared from the following raw materials in parts by weight: 600-1200 parts of a black silicate binder, 100-300 parts of a white silicate binder, 100-220 parts of expanded perlite, 500-1300 parts of expanded vermiculite, 10-35 parts of floating beads, 180-330 parts of mica, 1.5-5 parts of hydroxypropyl cellulose, 200-650 parts of ethylene vinyl acetate emulsion, 0.15-0.6 parts of sodium lauryl sulfate, 10-35 parts of a film-forming aid TX12, 3-8 parts of zirconium-containing aluminum silicate fiber, 3-10 parts of 1,2-propylene glycol, 20-80 parts of alumina fiber and 1500-3200 parts of water.

[0008] In some embodiments of the present invention, a fireproof and heat-insulating coating suitable for 500°C-800°C is provided, which is made of the following raw materials in parts by weight: 800-1000 parts of black silicate binder, 150-250 parts of white silicate binder, 120-220 parts of expanded perlite, 600-1000 parts of expanded vermiculite, 15-25 parts of floating beads, 190-250 parts of mica, 2-4 parts of hydroxypropyl cellulose, 280-450 parts of ethylene vinyl acetate emulsion, 0.18-0.35 parts of sodium lauryl sulfate, 18-28 parts of film-forming aid TX12, 3-5 parts of zirconium-containing aluminum silicate fiber, 4-8 parts of 1,2-propylene glycol, 40-60 parts of alumina fiber, and 2200-3000 parts of water.

[0009] In some embodiments of the present invention, a fireproof and heat-insulating coating suitable for 500°C-800°C is provided, which is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 154 parts of expanded perlite, 846 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 310 parts of ethylene vinyl acetate emulsion, 0.2 parts of sodium lauryl sulfate, 1222 parts of film-forming aid TX, 4 parts of zirconium-containing aluminum silicate fiber, 6 parts of 1,2-propylene glycol, 50 parts of alumina fiber, and 2710 parts of water.

[0010] In some embodiments of the present invention, the particle size of the expanded vermiculite is 150-3000 mesh.

[0011] In some embodiments of the present invention, the particle size of the expanded vermiculite is 200 mesh.

[0012] The invention discloses a method for preparing a fireproof and heat-insulating coating suitable for 500-800°C, comprising: preparing various raw materials in proportion, and mixing them evenly to obtain the coating.

[0013] The invention discloses an application of a 500-800°C fireproof and heat-insulating coating in the preparation of a 500-800°C fireproof and heat-insulating layer.

[0014] The invention discloses a fireproof and heat-insulating layer applicable to 500-800°C, which is obtained by spreading the fireproof and heat-insulating coating applicable to 500-800°C on a steel plate and naturally curing it for 28-40 days.

[0015] In some embodiments of the present invention, the steel plate has a size of 170 mm×170 mm×6 mm.

[0016] The applicant found that in the heating range of 400°C-1200°C, as the temperature increases, the overall volume trend of the white silicate binder is decreasing, while the overall volume trend of the black silicate binder is increasing. Relying on a single white silicate binder or a black silicate binder is not conducive to maintaining the volume stability of the fireproof and heat-insulating coating at high temperatures. Therefore, the present invention adopts a composite system of white silicate and black silicate binders.

[0017] The applicant found that as the temperature rises, the volume of basalt fiber gradually decreases, but the reduction is not obvious. When the temperature rises to around 1150°C, the volume of basalt fiber shrinks sharply. There are some risks when basalt is used as a refractory material. But it can be used as a reinforcing material for fire-retardant and heat-insulating coatings. During the heating process, as the temperature rises, the volume of mineral wool fiber expands, and then decreases and increases. When the temperature of mineral wool fiber exceeds about 950°C, the volume of mineral wool increases. The characteristics of mineral wool can be used, combined with the characteristics of the increase in temperature volume of black silicate, to prepare a fireproof and heat-insulating layer with a relatively stable volume. Between 400°C and 550°C, the volume of carbon fiber changes little, which shows that carbon fiber is relatively stable in this temperature range. When the temperature exceeds about 550°C, the linear pixel size of carbon fiber shrinks sharply. This shows that when the temperature reaches 550°C, carbon fiber cannot be used as a reinforcing material for fire-retardant coatings. During the entire heating process, the volume of zirconium-containing aluminum silicate fiber is relatively stable at high temperatures and can be used as a reinforcing material for fire-retardant and heat-insulating coatings.

[0018] The applicant found that the fragmentation of fireproof and heat-insulating coatings is one of the phenomena that leads to the failure of thermal protection or poor thermal protection of the fireproof and heat-insulating layer. The greater the degree of fragmentation, the worse the thermal insulation effect. This is because when it fragments or cracks, heat can directly enter the steel plate through the cracks or fissures, resulting in a poor thermal insulation effect of the fireproof and heat-insulating layer. The main reason for the fragmentation or cracking of the fireproof and heat-insulating layer is the ratio of perlite and vermiculite, which account for the majority of the volume. The applicant plotted the vermiculite-perlite ratio and the test time when the fireproof and heat-insulating layer steel plate reached 500°C, and found that: when the vermiculite-perlite ratio is less than 5.5, as the vermiculite-perlite ratio increases, the fire resistance of the fireproof and heat-insulating layer increases; when the vermiculite-perlite ratio is 5.5-6.0, the fire resistance of the fireproof and heat-insulating layer is the largest; when the vermiculite-perlite ratio is greater than 6.0, the fire resistance of the fireproof and heat-insulating layer slowly decreases.

[0019] This is because the bulk density of expanded vermiculite is heavier than that of expanded perlite. When the total mass remains unchanged, the heavier the proportion of vermiculite, the greater the density of the fireproof and heat-insulating layer, that is, the greater the vermiculite-perlite ratio, the greater the density of the fireproof and heat-insulating layer. When the vermiculite-perlite ratio is low, the density of the fireproof and heat-insulating layer is low, the strength of the fireproof door core board is low, and the core board is easy to break when burned at high temperature, so the fire resistance is poor. As the vermiculite-perlite ratio increases, the anti-fragmentation ability of the fireproof and heat-insulating layer is improved, and its fire resistance gradually increases. When the vermiculite-perlite ratio increases to a certain value, the fire resistance of the fireproof door core board gradually decreases. This is because, after the vermiculite-perlite ratio increases to a certain value, as the density of the fireproof door core board increases, the thermal conductivity increases, so the thermal insulation performance of the fireproof and heat-insulating layer decreases, so the fire resistance decreases instead.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention adopts a binder to improve the strength of the fireproof and heat-insulating coating;

[0022] 2. The present invention adopts mica to improve the ablation resistance of the fireproof and heat-insulating coating;

[0023] 3. The present invention reduces the amount of ethylene vinyl acetate emulsion used, reduces the smoke production of fireproof and heat-insulating coatings at high temperatures, and reduces toxicity;

[0024] 4. The present invention adopts zirconium-containing aluminum silicate fiber and aluminum oxide fiber to improve the anti-cracking performance of the fireproof and heat-insulating coating.

[0025] 5. The present invention optimizes the ratio of expanded vermiculite to expanded perlite to improve the anti-cracking performance of the fireproof and heat-insulating coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a temperature thermal conductivity diagram of the fireproof and heat-insulating layer of the test example of the present invention.

[0027] Figure 2 This is a temperature specific heat capacity curve of the fireproof and heat-insulating layer of the test example of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] This embodiment discloses the fireproof and heat-insulating coating of the present invention which is applicable to 500°C-800°C, and the specific composition is shown in Table 1:

[0031] Table 1 Composition of fire retardant and heat insulating coatings

[0032]

[0033] In this embodiment, the particle size of the expanded vermiculite is 200 meshes.

[0034] Prepare the raw materials according to the proportions in Table 1 and mix them evenly to obtain the fireproof and heat-insulating coating.

[0035] Example 2

[0036] This embodiment discloses the fireproof and heat-insulating coating of the present invention applicable to 500°C-800°C, and the specific composition is shown in Table 2:

[0037] Table 2 Composition of fire retardant and heat insulating coatings

[0038]

[0039]

[0040] In this embodiment, the particle size of the expanded vermiculite is 200 mesh.

[0041] Prepare the raw materials according to the proportions in Table 2 and mix them evenly to obtain the fireproof and heat-insulating coating.

[0042] Example 3

[0043] This embodiment discloses the fireproof and heat-insulating coating of the present invention applicable to 500°C-800°C, and the specific composition is shown in Table 3:

[0044] Table 3 Composition of fire retardant and heat insulating coatings

[0045]

[0046] In this embodiment, the particle size of the expanded vermiculite is 200 mesh.

[0047] Prepare the raw materials according to the proportions in Table 3 and mix them evenly to obtain the fireproof and heat-insulating coating.

[0048] Example 4

[0049] This embodiment discloses the fireproof and heat-insulating coating of the present invention applicable to 500°C-800°C, and the specific composition is shown in Table 4:

[0050] Table 3 Composition of fire retardant and heat insulating coatings

[0051]

[0052]

[0053] In this embodiment, the particle size of the expanded vermiculite is 200 mesh.

[0054] Prepare the raw materials according to the proportions in Table 4 and mix them evenly to obtain the fireproof and heat-insulating coating.

[0055] Test Case

[0056] The application of a fireproof and heat-insulating coating suitable for 500°C-800°C disclosed in Example 4 of the present invention in the preparation of a fireproof and heat-insulating layer suitable for 500°C-800°C.

[0057] The fireproof and heat-insulating coating prepared in Example 4 of the present invention was spread on a steel plate of 170 mm×170 mm×6 mm and naturally cured for 45 days to obtain a fireproof and heat-insulating layer suitable for 500°C-800°C.

[0058] The thermal conductivity (500°C, 600°C, 700°C, 800°C, 900°C, 1000°C), density, specific heat capacity, emissivity and absorption coefficient of the fireproof and heat-insulating layer were tested. The test structure is shown in Table 5.

[0059] Table 5 Test results

[0060]

[0061]

[0062] With temperature as the horizontal axis and thermal conductivity as the vertical axis, draw a temperature thermal conductivity diagram of the fireproof insulation layer, such as Figure 1 shown.

[0063] from Figure 1 It can be seen that the thermal conductivity is a temperature-varying function, which is a one-dimensional constant coefficient equation. The slope K is calculated as follows:

[0064] K(T)=(λT2-λT1) / (T2-T1)

[0065] Note: K(T): slope at temperature T; λT2: thermal conductivity at high temperature; λT1: thermal conductivity at high temperature; T2: temperature at low temperature; T1: temperature at low temperature.

[0066] The values ​​of T1 and T2 are 500°C and 1000°C respectively; the values ​​of λT1 and λT2 are 0.138W / m*K and 0.286W / m*K respectively.

[0067] Calculation shows that K = (0.286-0.138) / (1000-500) (W / m*K) / °C = 0.000296 (W / m*K) / °C.

[0068] Therefore, in the range of 500℃ to 1000℃, the thermal conductivity of the studied fire insulation layer is calculated as follows:

[0069] λ(T)=0.000296*TW / m*K

[0070] Where: T is temperature.

[0071] The thermal conductivity of the fireproof insulation layer increases with the change of temperature. The reasons are as follows:

[0072] (1) Crystal structure of the material: As the temperature rises, the vibration of atoms in the fireproof and heat-insulating crystals intensifies, resulting in more energy transfer, thereby increasing the thermal conductivity.

[0073] (2) Influence of refractory fillers and binders: Refractory fillers and binders may become more active as the temperature increases, resulting in changes in thermal conductivity.

[0074] (3) Molecular motion: At high temperatures, the thermal motion of the molecules in the fireproof insulation layer intensifies. The faster the molecular motion, the weaker the interaction between molecules. Therefore, the heat transfer is faster and the thermal conductivity is greater.

[0075] (4) Plasticity change of fireproof and heat-insulating layer: The increase in temperature will cause the plasticity change of the fireproof and heat-insulating layer, thereby affecting the thermal conductivity of the material.

[0076] With temperature as the horizontal axis and specific heat capacity as the vertical axis, draw a temperature specific heat capacity curve of the fireproof insulation layer, such as Figure 2 shown.

[0077] Depend on Figure 2 It can be seen that the specific heat capacity of the fireproof and heat-insulating layer is also a function of variable temperature.

[0078] When the temperature is less than about 80℃, the specific heat capacity of the fireproof and heat-insulating layer increases with the increase of temperature. This is because the fireproof and heat-insulating layer is a material with more closed-cell structures than open-cell structures. During the process of heating to about 80℃ at room temperature, the internal pressure of the fireproof and heat-insulating layer of the material increases, and the pressure of the furnace temperature causes the volume of the fireproof and heat-insulating layer to shrink, thereby increasing the density. The denser the material, the greater its specific heat capacity. This is because the greater the density, the greater the interaction force between molecules, and the more complex and diverse the energy transfer between molecules, so the greater the heat that needs to be absorbed.

[0079] When the temperature is between 80℃ and 150℃, the free water in the fireproof and heat-insulating layer will slowly evaporate and turn into gas, leaving the fireproof and heat-insulating layer, causing the fireproof and heat-insulating layer to become lighter and its density to decrease. Because the smaller the density, the smaller the interaction force between molecules, the smaller the energy transfer between molecules, and therefore the less heat to be absorbed. At the same time, as the temperature rises, the molecular vibration of the fireproof and heat-insulating layer intensifies, the molecular energy increases, and therefore the less heat to be absorbed.

[0080] When the temperature is between 150℃ and 300℃, the combined water inside the fireproof and heat-insulating layer absorbs heat, turns into gaseous water and is released into the atmosphere. Some organic molecules absorb heat and decompose, also absorbing heat, so the specific heat capacity increases slowly.

[0081] When the temperature exceeds 300°C, the sulfides in the inorganic binder in the fireproof and heat-insulating layer can decompose to produce sulfur dioxide gas, which is released and makes the mass of the fireproof and heat-insulating layer lighter, so the specific heat capacity slowly decreases.

[0082] In the range of 500° C. to 1000° C., the thermal conductivity of the fireproof and heat-insulating layer of the present invention is a temperature-varying function, which conforms to a one-dimensional constant coefficient equation.

[0083] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A fireproof and heat-insulating coating suitable for 500℃-800℃, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 600-1200 parts of black silicate binder, 100-300 parts of white silicate binder, 100-220 parts of expanded perlite, 500-1300 parts of expanded vermiculite, 10-35 parts of floating beads, 180-330 parts of mica, 1.5-5 parts of hydroxypropyl cellulose, 200-650 parts of ethylene vinyl acetate emulsion, 0.15-0.6 parts of sodium lauryl sulfate, 10-35 parts of film-forming aid TX12, 3-8 parts of zirconium-containing aluminum silicate fiber, 3-10 parts of 1,2-propylene glycol, 20-80 parts of alumina fiber and 1500-3200 parts of water.

2. According to claim 1, a fireproof and heat-insulating coating suitable for 500°C-800°C, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 800-1000 parts of black silicate binder, 150-250 parts of white silicate binder, 120-220 parts of expanded perlite, 600-1000 parts of expanded vermiculite, 15-25 parts of floating beads, 190-250 parts of mica, 2-4 parts of hydroxypropyl cellulose, 280-450 parts of ethylene vinyl acetate emulsion, 0.18-0.35 parts of sodium lauryl sulfate, 18-28 parts of film-forming aid TX12, 3-5 parts of zirconium-containing aluminum silicate fiber, 4-8 parts of 1,2-propylene glycol, 40-60 parts of alumina fiber and 2200-3000 parts of water.

3. The fireproof and heat-insulating coating suitable for 500°C-800°C according to claim 1, It is characterized in that The invention is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 154 parts of expanded perlite, 846 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 310 parts of ethylene vinyl acetate emulsion, 0.2 parts of sodium lauryl sulfate, 1222 parts of film-forming aid TX, 4 parts of zirconium-containing aluminum silicate fiber, 6 parts of 1,2-propylene glycol, 50 parts of alumina fiber and 2710 parts of water.

4. The fireproof and heat-insulating coating suitable for 500°C-800°C according to claim 1, It is characterized in that The particle size of the expanded vermiculite is 150-3000 meshes.

5. The fireproof and heat-insulating coating suitable for 500°C-800°C according to claim 4, It is characterized in that The particle size of the expanded vermiculite is 200 meshes.

6. A method for preparing a fireproof and heat-insulating coating suitable for 500°C-800°C according to any one of claims 1 to 5, It is characterized in that include: Prepare the raw materials in proportion and mix them evenly.

7. Use of the fireproof and heat-insulating coating suitable for 500°C-800°C according to claims 1 to 5 in preparing a fireproof and heat-insulating layer suitable for 500°C-800°C.

8. A fireproof and heat-insulating layer suitable for 500℃-800℃, It is characterized in that The fireproof and heat-insulating coating suitable for 500-800°C as described in any one of claims 1 to 5 is spread on a steel plate and naturally cured for 28 to 40 days to obtain the coating.

9. A fireproof and heat-insulating layer suitable for 500°C-800°C according to claim 8, It is characterized in that The size of the steel plate is 170 mm×170 mm×6 mm.

Citation Information

Patent Citations

  • External wall weather-resistant fine putty powder and preparation method therefor

    CN105036642A

  • Inorganic coating and preparation method thereof

    CN107200525A

  • Thick steel structure fireproof coating agent and preparation method thereof

    CN117069439A

  • Non expansion type steel structure fire retarding anticorrosion paint

    CN1948404A

  • Heat insulation structure

    JP2008291644A