Conductive ink, preparation method thereof and preparation method of wearable electronic device

Through the combination of liquid metal, eutectic solvent and tannin, a protective shell and hydrogen bond network is formed, which solves the problems of oxidation and low conductivity of conductive ink, and improves conductivity and stability, and is suitable for wearable electronics. Preparation of devices.

CN119019890APending Publication Date: 2024-11-26SUZHOU UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411158175.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing conductive inks are prone to oxidation and have low conductivity, and cannot achieve crack-free surfaces under wet conditions, resulting in insufficient stability and performance in applications.

Method used

Using a combination of liquid metal, eutectic solvent and tannin acid, the protective shell is formed by crosslinking the carboxyl groups in the eutectic solvent with the metal ion of the liquid metal to prevent oxidation and the formation of hydrogen bond network through hydroxyl groups. The dispersion of liquid metals can improve conductivity and adhesion.

Benefits of technology

It significantly improves the conductivity and stability of conductive inks, prevents oxidation, enhances the dispersion and adhesion of liquid metals, and ensures high performance under wet conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019890A_ABST
    Figure CN119019890A_ABST
Patent Text Reader

Abstract

The invention provides conductive ink and a preparation method thereof, and a preparation method of a wearable electronic device, and relates to the technical field of material chemistry. The conductive ink comprises a liquid metal, a deep eutectic solvent and tannic acid, the deep eutectic solvent is coordinated with the liquid metal, the deep eutectic solvent is further used for forming a polymer network and a hydrogen bond network, the tannic acid is coordinated with the liquid metal, the tannic acid reacts with the deep eutectic solvent to form an enhanced hydrogen bond network, and the enhanced hydrogen bond network is further used for forming a polymer network. The hydrogen bond network is used for dispersing the liquid metal. According to the conductive ink disclosed by the invention, the oxidation resistance of the conductive ink is improved by utilizing the protective shell formed by the eutectic solvent and the liquid metal, and the conductivity of the conductive ink is improved by utilizing a hydrogen bond network and an enhanced hydrogen bond network formed in the conductive ink.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material chemistry, and in particular to a conductive ink and a preparation method thereof, and a preparation method of a wearable electronic device. Background Art

[0002] Conductive ink is made of various conductive fillers, has certain conductive properties, and can be used in various printing inks. At present, as a kind of highly functional conductive material, conductive ink has become an important material used in printed circuit technology, semiconductor technology, printed electronic devices and other processes. Liquid metal is widely used in the preparation of conductive ink due to its high electrical and thermal conductivity, low mechanical properties and viscosity, and unique liquid properties.

[0003] However, since liquid metal has significant surface tension, it tends to aggregate to form low surface energy balls, resulting in low dispersion of liquid metal in conductive ink, and the liquid metal on the surface of conductive ink is easily oxidized, thereby affecting the conductive properties of the conductive ink. In the prior art, liquid metal in conductive ink is usually encapsulated using thiol surfactants, which can effectively avoid the oxidation of liquid metal in conductive ink. However, since thiol surfactants themselves do not have conductive properties, the conductivity of conductive inks dispersed using thiol surfactants is usually low, and the encapsulated liquid metal nanoparticles still lack sufficient antioxidant capacity, and cannot achieve a wide range of crack-free surfaces under humid conditions. Summary of the invention

[0004] An object of the first aspect of the present invention is to provide a conductive ink to solve the technical problem in the prior art that the conductive ink is easily oxidized and has low conductivity.

[0005] Another object of the first aspect of the present invention is to improve the adhesion of the conductive ink.

[0006] The second aspect of the present invention aims to provide a method for preparing a conductive ink, which is used to prepare the conductive ink.

[0007] The third aspect of the present invention aims to provide a method for preparing a wearable electronic device based on conductive ink.

[0008] According to the purpose of the first aspect of the present invention, the present invention provides a conductive ink, comprising:

[0009] Liquid metal;

[0010] A deep eutectic solvent coordinated with the liquid metal, the deep eutectic solvent also being used to form a polymer network and a hydrogen bond network;

[0011] Tannic acid is coordinated with the liquid metal. The tannic acid reacts with the low eutectic solvent to form an enhanced hydrogen bond network, and the enhanced hydrogen bond network is used to disperse the liquid metal.

[0012] Optionally, the low eutectic solvent comprises a first reagent containing a hydrogen bond donor and a second reagent containing a hydrogen bond acceptor, and the first reagent and the second reagent are used to form the hydrogen bond network.

[0013] Optionally, the molar ratio of the first reagent to the second reagent is any value in the range of 2:0.5-2:2.

[0014] Optionally, the mass ratio of the tannic acid to the first reagent is any value in the range of 2%-30%.

[0015] Optionally, the first reagent includes any one of lipoic acid, acrylic acid, acrylamide or ethylene glycol, and the second reagent includes any one of choline chloride, betaine, ethanolamine or mercaptoethanol.

[0016] Optionally, the mass ratio of the low eutectic solvent to the liquid metal is any value in the range of 0.05:1-0.5:1.

[0017] Optionally, the liquid metal includes any one of a gallium-indium alloy, a gallium-indium-tin alloy, a gallium-zinc alloy or a bismuth-tin alloy.

[0018] According to the purpose of the second aspect of the present invention, the present invention also provides a method for preparing a conductive ink, which is used to prepare a conductive ink as described in any one of the above items, and the preparation method comprises the following steps:

[0019] Adding a first reagent and a second reagent having a preset molar ratio into a solvent, and reacting at a preset temperature to prepare a deep eutectic solvent;

[0020] Adding tannic acid to the deep eutectic solvent and mixing well to prepare a polymer solution;

[0021] adding liquid metal to the solvent, and sequentially performing ultrasonic mixing, suspension centrifugation and concentration to prepare a liquid metal concentrate;

[0022] The polymer solution is added into the liquid metal concentrate, and the mixture is evenly mixed to prepare the conductive ink.

[0023] According to the third aspect of the present invention, the present invention further provides a method for preparing a wearable electronic device based on conductive ink, wherein the conductive ink comprises any one of the conductive inks described above, and the method for preparing the wearable electronic device comprises the following steps:

[0024] Preparing a first flexible film;

[0025] Coating the conductive ink on the surface of the flexible film to form a patterned circuit;

[0026] Coating a low eutectic solvent on the surface of the patterned circuit and forming a second flexible film after solidification;

[0027] The first flexible film and the second flexible film are separated, and the patterned circuit on the surface of the second flexible film is sintered and connected with wires in sequence, and then packaged to obtain the wearable electronic device.

[0028] The invention comprises liquid metal, a low eutectic solvent and tannic acid, wherein the low eutectic solvent comprises a large number of carboxyl groups and hydroxyl groups, and the carboxyl groups undergo cross-linking and coordination reactions with metal ions in the liquid metal to form a protective shell on the surface of the liquid metal to prevent oxidation of the surface of the conductive ink, thereby improving the stability of the conductive ink in the air, and the hydrogen bond network formed between the hydroxyl groups also helps the dispersion of the low eutectic solvent in the liquid metal, thereby improving the dispersibility of the liquid metal in the conductive ink, and further improving the conductivity of the conductive ink. At the same time, tannic acid contains a large number of hydroxyl groups, and tannic acid forms an enhanced hydrogen bond network with the hydrogen bond network in the low eutectic solvent to further improve the dispersibility of the liquid metal in the conductive ink, thereby further improving the conductivity of the conductive ink.

[0029] Furthermore, the molar ratio of the first agent to the second agent in the conductive ink of the present invention is any value in the range of 2:0.5-2:2, that is, when the molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is any value in the range of 2:0.5-2:2, a hydrogen bond network with higher stability is formed in the low eutectic solvent, thereby improving the dispersibility and adhesion of the liquid metal in the conductive ink.

[0030] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Hereinafter, some specific embodiments of the present invention will be described in detail in an exemplary and non-limiting manner with reference to the accompanying drawings. The same reference numerals in the accompanying drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the accompanying drawings:

[0032] Figure 1 is a schematic flow chart of a method for preparing a conductive ink according to an embodiment of the present invention;

[0033] Figure 2 is a schematic flow chart of a method for preparing a wearable electronic device according to an embodiment of the present invention;

[0034] Figure 3 is a schematic structural diagram of a wearable electronic device according to an embodiment of the present invention;

[0035] Figure 4 is a result diagram of an electrical performance test of a wearable electronic device according to an embodiment of the present invention;

[0036] Figure 5 4 is a result diagram of human motion monitoring by a wearable electronic device according to an embodiment of the present invention.

[0037] Reference numerals:

[0038] 100-wearable electronic device, 10-second flexible film, 20-patterned circuit. DETAILED DESCRIPTION

[0039] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0040] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. It is to be understood that the specific embodiments described herein are only used to explain the present application, rather than to limit the present application. It should also be noted that, for ease of description, only some structures related to the present application are shown in the accompanying drawings, rather than all structures. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0041] The terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.

[0042] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0043] The present invention provides a conductive ink. The conductive ink includes liquid metal, a low eutectic solvent and tannic acid, the low eutectic solvent is coordinated with the liquid metal, the low eutectic solvent is also used to form a polymer network and a hydrogen bond network, the tannic acid is coordinated with the liquid metal, the tannic acid reacts with the low eutectic solvent to form an enhanced hydrogen bond network, and the enhanced hydrogen bond network is used to disperse the liquid metal. Here, the polymer network formed by the low eutectic solvent can increase the flexibility of the conductive ink, improve the dispersibility of the liquid metal, and thus improve the conductivity of the conductive ink.

[0044] In this embodiment, the conductive ink includes liquid metal, a low eutectic solvent and tannic acid. The low eutectic solvent includes a large number of carboxyl groups and hydroxyl groups. The carboxyl groups undergo cross-linking and coordination reactions with metal ions in the liquid metal to form a protective shell on the surface of the liquid metal to prevent oxidation of the surface of the conductive ink, thereby improving the stability of the conductive ink in the air. The hydrogen bond network formed between the hydroxyl groups also helps to disperse the low eutectic solvent in the liquid metal, thereby improving the dispersibility of the liquid metal in the conductive ink, and further improving the conductivity of the conductive ink. At the same time, tannic acid contains a large number of hydroxyl groups, and tannic acid forms an enhanced hydrogen bond network with the hydrogen bond network in the low eutectic solvent to further improve the dispersibility of the liquid metal in the conductive ink, thereby further improving the conductivity of the conductive ink.

[0045] In this embodiment, the mechanical robustness and low oxygen permeability of the protective shell formed by the carboxyl groups in the low eutectic solvent and the liquid metal allow the conductive ink to remain stable in the air, avoiding the aggregation of the liquid metal and preventing the oxidation of the liquid metal, thereby reducing the difficulty of storing the conductive ink. Here, the carboxyl groups combine with the metal ions in the liquid metal to form ionic bonds, which can transfer charges between the liquid metal and the low eutectic solvent, thereby further improving the conductivity of the conductive ink.

[0046] In a further embodiment, the low eutectic solvent includes a first reagent containing a hydrogen bond donor and a second reagent containing a hydrogen bond acceptor, and the first reagent and the second reagent are used to form a hydrogen bond network. The formation of the hydrogen bond network can significantly enhance the stability of the liquid metal, while improving the structural rigidity of the conductive ink, which is beneficial to maintaining the shape and structure of the conductive ink and preventing deformation or damage under external stress. In addition, the formation of the hydrogen bond network can carry out charge transfer together with the liquid metal, thereby improving the conductivity of the conductive ink.

[0047] In a further embodiment, the molar ratio of the first reagent to the second reagent is any value in the range of 2:0.8-2:2. That is, the molar ratio of the first reagent to the second reagent can be 2:0.5, 2:0.6, 2:0.7, 2:0.8, 2:0.85, 2:0.9, 2:0.95, 2:1, 2:1.2, 2:1.4, 2:1.6, 2:1.8 or 2:2, or it can be any value in the range of 2:0.5-2:2. In other words, when the molar ratio of the first reagent to the second reagent is any value in the range of 2:0.5-2:2, that is, when the molar ratio of the hydrogen bond donor and the hydrogen bond acceptor is any value in 2:0.5-2:2, a hydrogen bond network with higher stability is formed in the low eutectic solvent, thereby improving the dispersibility and adhesion of the liquid metal in the conductive ink. In a preferred embodiment, the molar ratio of the hydrogen bond donor and the hydrogen bond acceptor is 2:1.

[0048] In a further embodiment, the mass ratio of tannic acid to the first reagent is in the range of 2% to

[0049] 30%. That is, the mass ratio between tannic acid and the first reagent can be 2%, 4%, 6%, 8%, 10%, 12%, 14%, 18%, 20%, 24%, 28% or 30%, or it can be any value in the range of 2%-30%. In the present embodiment, tannic acid includes a large number of phenolic hydroxyl groups, which further form a hydrogen bond network by combining with the hydrogen bonds in the first reagent, that is, the hydrogen bond network formed between tannic acid and the first reagent can further expand the hydrogen bond network in the low eutectic solvent, thereby forming an enhanced hydrogen bond network in the conductive ink. In other words, when the mass ratio between tannic acid and the first reagent is any value in the range of 2%-30%, the enhanced hydrogen bond network formed by tannic acid in the conductive ink can improve the stability and adhesion of the conductive ink, thereby improving the adhesion between the conductive ink and the printing medium, and avoiding shedding or peeling between the conductive ink and the substrate. At the same time, the enhanced hydrogen bond network can also improve the dispersion of liquid metal in the conductive ink and improve the weather resistance of the conductive ink, thereby improving the conductivity of the conductive ink while ensuring the performance stability of the conductive ink.

[0050] In a further embodiment, the first reagent includes any one of lipoic acid, acrylic acid, acrylamide or ethylene glycol, and the second reagent includes any one of choline chloride, betaine, ethanolamine or mercaptoethanol. In this embodiment, the first reagent can be any one of lipoic acid, acrylic acid, acrylamide or ethylene glycol, and the second reagent can be any one of choline chloride, betaine, ethanolamine or mercaptoethanol, that is, lipoic acid, acrylic acid, acrylamide and ethylene glycol are used as hydrogen bond donors, and choline chloride, betaine, ethanolamine and mercaptoethanol are used as hydrogen bond acceptors, and any hydrogen bond donor can react with any hydrogen bond acceptor to form a hydrogen bond network to improve the dispersibility of liquid metal in conductive ink.

[0051] In a preferred embodiment, the first reagent is thioctic acid, and the second reagent is choline chloride, that is, the hydrogen bond donor is thioctic acid, and the hydrogen bond acceptor is choline chloride. The five-membered ring containing disulfide bonds in thioctic acid undergoes thermally initiated ring-opening polymerization due to dynamic disulfide bond exchange to provide a large number of disulfide bonds for stabilizing the dispersibility of the liquid metal. At the same time, a stable hydrogen bond network is formed between thioctic acid and choline chloride, thereby improving the dispersibility of the liquid metal. The protective shell formed by the coordination of the hydroxyl group in thioctic acid and the metal ion in the liquid metal can prevent the surface of the conductive ink from being oxidized, thereby ensuring the storage stability of the conductive ink.

[0052] In a further embodiment, the mass ratio of the low eutectic solvent to the liquid metal is any value in the range of 0.05:1-0.5:1. That is, the mass ratio of the low eutectic solvent to the liquid metal can be 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1 or 0.5:1, or any value in the range of 0.05:1-0.5:1. In this embodiment, when the mass ratio of the low eutectic solvent to the liquid metal is any value in the range of 0.05:1-0.5:1, a stable hydrogen bond network is formed in the low eutectic solvent to improve the dispersibility of the liquid metal in the conductive ink, and the carboxyl group in the low eutectic solvent is sufficient to coordinate with the liquid metal on the surface of the conductive ink to form a stable protective shell on the surface of the conductive ink to avoid oxidation of the surface of the conductive ink, thereby improving the stability of the conductive ink.

[0053] In a further embodiment, the liquid metal includes any one of a gallium-indium alloy, a gallium-indium-tin alloy, a gallium-zinc alloy or a bismuth-tin alloy. In this embodiment, the metal ions (for example, gallium ions or bismuth ions) in the liquid metal form a stable protective layer with the hydroxyl groups in the low eutectic solvent, and the hydrogen bond network in the low eutectic solvent and the enhanced hydrogen bond network formed between tannic acid and the low eutectic solvent act together on the liquid metal, thereby improving the dispersibility of the liquid metal in the conductive ink. In a preferred embodiment, the liquid metal is a gallium-indium alloy.

[0054] Figure 1 is a schematic flow chart of a method for preparing a conductive ink according to an embodiment of the present invention.

[0055] like Figure 1 As shown, the present invention also provides a method for preparing a conductive ink, which is used to prepare a conductive ink including any one of the above items, and the preparation method comprises the following steps:

[0056] Step S100: adding a first reagent and a second reagent having a preset molar ratio into a solvent, and reacting at a preset temperature to prepare a deep eutectic solvent;

[0057] Step S200: adding tannic acid to the deep eutectic solvent and mixing well to prepare a polymer solution;

[0058] Step S300: adding liquid metal to a solvent, and sequentially performing ultrasonic mixing, suspension centrifugation and concentration to prepare a liquid metal concentrate;

[0059] Step S400: adding the polymer solution to the liquid metal concentrate, and mixing them evenly to prepare a conductive ink.

[0060] In this embodiment, a low eutectic solvent is prepared by dissolving the first reagent and the second reagent in a solvent under preset reaction temperature conditions, a polymer solution is prepared by reacting tannic acid with the low eutectic solvent, a liquid metal concentrate is prepared and the liquid metal concentrate is mixed with the polymer solution to prepare a conductive ink having a protective shell and higher conductivity.

[0061] In step S100, the preset molar ratio is any value in the range of 2:0.5-2:2, the solvent is anhydrous ethanol, the preset temperature is any value in the range of 85°C-95°C, and the reaction time of the first reagent and the second reagent is any value in the range of 8min-15min. That is, the first reagent and the second reagent are dissolved in anhydrous ethanol under the preset temperature conditions to form a low eutectic solvent that is evenly mixed. Here, the preparation of the low eutectic solvent is carried out under sealed conditions to reduce the volatilization of anhydrous ethanol.

[0062] In the present embodiment, the preset temperature is any value in the range of 85°C-95°C, and the reaction time of the first reagent and the second reagent is any value in the range of 8min-15min, that is, the preset temperature can be 85°C, 87°C, 89°C, 90°C, 91°C, 92°C, 93°C or 95°C, or any value in the range of 85°C-95°C, and the reaction time of the first reagent and the second reagent can be 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min, or any value in the range of 8min-15min. In the present embodiment, the reaction time and the preset temperature are within the above range, which can ensure that the first reagent and the second reagent are completely dissolved in anhydrous ethanol, and at the same time accelerate the dissolution rate of the first reagent and the second reagent, and prevent the reaction temperature from being too high, causing the first reagent and the second reagent to have a side reaction, or the reaction time is too long, causing more solvent volatilization.

[0063] Before step S200, the method for preparing the conductive ink further includes:

[0064] Step S210: adding tannic acid into anhydrous ethanol to prepare a tannic acid solution.

[0065] In step S300, the solvent is anhydrous ethanol, the ultrasonic power is any value in the range of 300W-600W, and the ultrasonic time is any value in the range of 5min-45min, so as to ultrasonically decompose the liquid metal into a liquid metal dispersion, the particle size of the liquid metal particles in the liquid metal dispersion is any value in the range of 180nm-220nm, and the liquid metal concentrate with a mass fraction in the range of 70wt.%-95wt.% is prepared by suspension centrifugation and concentration. That is to say, the ultrasonic power in this embodiment can be 300W, 350W, 400W, 450W, 500W, 550W or 600W, or any value in the range of 300W-600W, and the ultrasonic time can be 5min, 10min, 15min, 20min, 25min, 30min, 35min, 40min or 45min, or any value in the range of 5min-45min, to prepare a liquid metal dispersion with a particle size of liquid metal particles in the range of 180nm-220nm, so that the liquid metal has better dispersibility in the conductive ink. Here, the particle size of the liquid metal particles in the liquid metal dispersion can be 180nm, 190nm, 200nm, 180nm or 180nm, or any value in the range of 180nm-220nm. The mass fraction of the liquid metal in the liquid metal concentrate can be 70wt.%, 75wt.%, 80wt.%, 85wt.%, 90wt.% or 95wt.%, or any value in the range of 70wt.%-95wt.%.

[0066] Figure 2 is a schematic flow chart of a method for preparing a wearable electronic device according to an embodiment of the present invention.

[0067] like Figure 2 As shown, the present invention also provides a method for preparing a wearable electronic device 100 based on conductive ink, wherein the conductive ink includes any of the conductive inks described above, and the method for preparing the wearable electronic device 100 includes the following steps:

[0068] Step S500: preparing a first flexible film;

[0069] Step S600: coating a conductive ink on the surface of the flexible film to form a patterned circuit 20;

[0070] Step S700: coating a low eutectic solvent on the surface of the patterned circuit 20 and curing and forming the second flexible film 10;

[0071] Step S800: separating the first flexible film and the second flexible film 10, and sequentially sintering and connecting the patterned circuit 20 on the surface of the second flexible film 10, and packaging to obtain the wearable electronic device 100.

[0072] In this embodiment, a patterned circuit 20 having a preset pattern is formed by coating a conductive ink on a template on the surface of a first flexible film, and a low eutectic solvent is coated on the surface of the first flexible film to form a second flexible film 10 on the surface of the patterned circuit 20. Since the patterned circuit 20 and the second flexible film 10 have a stronger adhesion force, the second flexible film 10 drives the patterned circuit 20 to be peeled off from the surface of the first flexible film when the second flexible film 10 is separated from the first flexible film, and the patterned circuit 20 is sequentially sintered, connected with wires, and packaged to prepare a wearable electronic device 100 having higher conductivity and better adhesion performance. Here, the first flexible film includes any one of polydimethylsiloxane, polyethylene terephthalate, and thermoplastic polyurethane.

[0073] Figure 3 is a schematic structural diagram of a wearable electronic device according to an embodiment of the present invention.

[0074] like Figure 3 As shown, in this embodiment, the wearable electronic device 100 includes a patterned circuit 20 and two second flexible films 10 .

[0075] Figure 4 is a result diagram of an electrical performance test of a wearable electronic device according to an embodiment of the present invention, Figure 5 4 is a result diagram of human motion monitoring by a wearable electronic device according to an embodiment of the present invention.

[0076] In order to verify the sensing performance and adhesion of the wearable electronic device 100 in this embodiment, the sensing performance and adhesion of the wearable device in this embodiment are tested, and the following results are obtained: Figure 4 and Figure 5 The test results are shown.

[0077] like Figure 4 As shown, the electrical sensing performance of the wearable electronic device 100 was tested under strain conditions of 30%, 60% and 90%, and stable electrical signal changes were detected, indicating that the liquid metal wearable electronic device 100 prepared in this embodiment has stable electrical sensing performance.

[0078] like Figure 5 As shown, the wearable electronic device 100 can monitor continuous and stable signals of human joint movement, indicating that the wearable electronic device 100 prepared in this embodiment has good conductivity and reflects the amplitude of human movement through the strength of the electrical signal, thereby reminding the athlete to adjust the exercise posture in a standardized manner.

[0079] In step S800, the patterned circuit 20 is sintered to destroy the liquid metal oxide layer on the surface of the conductive ink, so that the liquid metal inside the liquid metal particles flows out, thereby achieving the conduction of the patterned circuit 20. Here, the method of achieving the conduction of the patterned circuit 20 also includes any one of pasting and peeling, laser irradiation, and pressing.

[0080] In some embodiments, a first reagent and a second reagent with a preset molar ratio of 2:0.5-2:2 are first added to anhydrous ethanol, reacted at 85°C-95°C to prepare a low eutectic solvent, tannic acid is added to the low eutectic solvent, mixed evenly to prepare a polymer solution, in which the mass ratio of tannic acid to the first reagent is any value between 2% and 30%, liquid metal is added to anhydrous ethanol, ultrasonic mixing, suspension centrifugation and concentration are performed in sequence to prepare a liquid metal concentrate, the polymer solution is added to the liquid metal concentrate, mixed evenly to prepare a conductive ink.

[0081] The present application will be further described in detail below with reference to specific embodiments.

[0082] Embodiment 1

[0083] In this embodiment, lipoic acid and choline chloride in a molar ratio of 2:1 are first dissolved in anhydrous ethanol, reacted at 90°C to prepare a low eutectic solvent, tannic acid is added to the low eutectic solvent, mixed evenly to prepare a polymer solution, the mass ratio of tannic acid to lipoic acid in the polymer solution is 10%, gallium-indium alloy is added to anhydrous ethanol, ultrasonicated for 30 minutes under an ultrasonic power of 450W, and suspended centrifuged and concentrated to prepare a gallium-indium alloy concentrate with a mass fraction of 90wt.%, the polymer solution is added to the gallium-indium alloy concentrate, mixed evenly to prepare a conductive ink. The conductivity of the conductive ink in this embodiment is 10 6 S / m.

[0084] Comparative Example 1

[0085] The difference between this embodiment and the first embodiment is that the molar ratio of lipoic acid to choline chloride in this embodiment is 0.5, and the conductivity of the conductive ink in this embodiment is 10 3 S / m.

[0086] Comparative Example 2

[0087] The difference between this embodiment and the first embodiment is that the molar ratio of lipoic acid to choline chloride in this embodiment is 3, and the conductivity of the conductive ink in this embodiment is 10 S / m.

[0088] Comparative Example 3

[0089] The difference between this embodiment and the first embodiment is that the mass ratio of tannic acid to lipoic acid in this embodiment is 1%, and the conductivity of the conductive ink in this embodiment is 10 2 S / m.

[0090] Comparative Example 4

[0091] The difference between this embodiment and the first embodiment is that the mass ratio of tannic acid to lipoic acid in this embodiment is 35%, and the conductivity of the conductive ink in this embodiment is 10 3 S / m.

[0092] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A conductive ink, characterized in that: include: Liquid metal; A deep eutectic solvent coordinated with the liquid metal, the deep eutectic solvent also being used to form a polymer network and a hydrogen bond network; Tannic acid is coordinated with the liquid metal. The tannic acid reacts with the low eutectic solvent to form an enhanced hydrogen bond network, and the hydrogen bond network is used to disperse the liquid metal.

2. The conductive ink according to claim 1, characterized in that: The deep eutectic solvent comprises a first reagent containing a hydrogen bond donor and a second reagent containing a hydrogen bond acceptor, and the first reagent and the second reagent are used to form the hydrogen bond network.

3. The conductive ink according to claim 2, characterized in that: The molar ratio of the first reagent to the second reagent is any value in the range of 2:0.5-2:

2.

4. The conductive ink according to claim 3, characterized in that: The mass ratio of the tannic acid to the first reagent is any value in the range of 2%-30%.

5. The conductive ink according to claim 4, characterized in that: The first reagent includes any one of lipoic acid, acrylic acid, acrylamide or ethylene glycol, and the second reagent includes any one of choline chloride, betaine, ethanolamine or mercaptoethanol.

6. The conductive ink according to claim 5, characterized in that: The mass ratio of the deep eutectic solvent to the liquid metal is any value in the range of 0.05:1-0.5:

1.

7. The conductive ink according to any one of claims 1 to 6, characterized in that: The liquid metal includes any one of a gallium-indium alloy, a gallium-indium-tin alloy, a gallium-zinc alloy or a bismuth-tin alloy.

8. A method for preparing a conductive ink, for preparing the conductive ink according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Adding a first reagent and a second reagent having a preset molar ratio into a solvent, and reacting at a preset temperature to prepare a deep eutectic solvent; Adding tannic acid to the deep eutectic solvent and mixing well to prepare a polymer solution; adding liquid metal to the solvent, and sequentially performing ultrasonic mixing, suspension centrifugation and concentration to prepare a liquid metal concentrate; The polymer solution is added into the liquid metal concentrate, and the mixture is evenly mixed to prepare the conductive ink.

9. A method for preparing a wearable electronic device based on conductive ink, characterized in that: The conductive ink comprises the conductive ink described in any one of claims 1 to 7, and the preparation method of the wearable electronic device 100 comprises the following steps: Preparing a first flexible film; Coating the conductive ink on the surface of the flexible film to form a patterned circuit; Coating a low eutectic solvent on the surface of the patterned circuit and forming a second flexible film after solidification; The first flexible film and the second flexible film are separated, and the patterned circuit on the surface of the second flexible film is sintered and connected with wires in sequence, and then packaged to obtain the wearable electronic device.

Citation Information

Cited By

  • Conductive hot melt adhesive with near-infrared light welding characteristic and preparation method thereof

    CN119639415A

  • Conductive hot melt adhesive having near-infrared light welding characteristics and preparation method thereof

    US12767863B2