Two-component waterborne epoxy floor coating capable of degrading automobile exhaust and preparation method of two-component waterborne epoxy floor coating

By using hydrophilic silicon-based porous materials and modified TiO2 with load-modified titanium dioxide in floor coatings, the problem that the existing technology cannot effectively remove automobile exhaust is solved, and efficient air purification and environmentally friendly coating solutions are achieved. .

CN119019912APending Publication Date: 2024-11-26CHANGSHA BIAOLANG LIVING TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411291645.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing floor coatings cannot effectively degrade and purify car exhaust in underground garages, resulting in air pollution and health risks, and most oily coatings contain solvents that are harmful to the environment and the human body.

Method used

Two-component water-based epoxy floor coating, hydrophilic silicon-based porous material containing load-modified titanium dioxide as decomposition functional material, and decomposes CO, CH and nitrogen oxide compounds under visible light by modifying TiO2, and passes through epoxy dioxide. The film formation process of the grade dispersion changes the paint film from hydrophilic to hydrophobic, and moves directionally to the surface of the paint film, improving the friction resistance of the coating.

Benefits of technology

It has achieved efficient removal of CO, CH and nitrogen oxide compounds in automobile exhaust, with 24-hour removal rates of 63.1%, 70.5%, and 71.2%, respectively, and has no irritating odor during construction, reducing the harm to the environment and the human body. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044780510000081
    Figure BDA0005044780510000081
Patent Text Reader

Abstract

The invention discloses a two-component waterborne epoxy floor coating capable of degrading automobile exhaust and a preparation method of the two-component waterborne epoxy floor coating. A component A comprises deionized water, a waterborne epoxy curing agent, pigment filler, a dispersing agent, a defoaming agent, a wetting leveling agent, an anti-settling agent and a decomposition material, and the decomposition material is a hydrophilic silicon-based porous material loaded with modified titanium dioxide; the component B comprises a water-based epoxy emulsion, deionized water and a water-based auxiliary agent, and the weight ratio of the component A to the component B is 2.5: 1. The two-component waterborne epoxy floor coating capable of degrading the automobile exhaust solves the problem that harmful gas cannot be captured due to the fact that a decomposition material is sealed by a paint film, and the provided two-component waterborne epoxy floor coating capable of degrading the automobile exhaust is low in odor, environmentally friendly in construction, capable of effectively degrading harmful ingredients such as hydrocarbon and nitric oxide in the automobile exhaust into non-toxic and harmless substances after construction and capable of effectively degrading the harmful ingredients in the automobile exhaust into non-toxic and harmless substances. Wear resistance, corrosion resistance and the like reach industrial standards, and the material is particularly suitable for underground garages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of coatings, and in particular relates to a two-component water-based epoxy floor coating capable of degrading automobile exhaust and a preparation method thereof. Background Art

[0002] Floor paint is a kind of coating that can firmly cover the surface of objects for protection, decoration and marking. It is mainly used in factories, underground garages, etc. When it is used in underground garages, the ventilation is poor, the solvent evaporates after construction and is difficult to be discharged, and the garage has a heavy odor, which makes it difficult to put the underground garage into use in time; in addition, during use, a large amount of exhaust gas discharged when the car is started is accumulated in the underground garage and cannot be effectively discharged in time. Automobile exhaust mainly contains CO, CH, NO X and some solid particles. CO has the highest content, which causes tissue hypoxia, resulting in symptoms such as headaches, and in severe cases, suffocation and death. There are more than 200 types of CH, including 32 types of polycyclic aromatic hydrocarbons, which are prone to cause lung cancer. NO X It is highly toxic and can cause diseases such as emphysema.

[0003] At present, most of the floor coatings on the market are oily and contain a lot of solvents. Solvents pollute the environment and are harmful to the human body. A small number of oil-to-water floor coatings basically do not affect the environment and are less toxic to the construction workers, but they cannot purify the air. In underground garages, where air circulation is poor and car exhaust is concentrated, the floor coatings on the market currently have no degradation or purification capabilities.

[0004] Therefore, in view of the current environmental protection and health needs, how to provide a non-toxic floor coating with purification ability is an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0005] In view of this, the present invention provides a two-component water-based epoxy floor paint capable of degrading automobile exhaust. The floor paint has excellent degradation function on automobile exhaust and has no irritating odor during construction.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A two-component water-based epoxy floor coating capable of degrading automobile exhaust, comprising the following components by weight percentage:

[0008] Component A: deionized water 20-40%, water-based epoxy curing agent 30-50%, pigment and filler 20-50%, dispersant 0.1-1%, defoamer 0.1%-0.3%, wetting and leveling agent 0.1-1%, anti-settling agent 0.1-0.5%, decomposition functional material 3-10%;

[0009] Component B: 50-80% water-based epoxy emulsion, 20-40% deionized water, 1-3% water-based additive;

[0010] The weight ratio of the A component to the B component is 2.5:1.

[0011] Preferably, the filler in the color filler is one or more of barium sulfate, rutile titanium dioxide, calcined kaolin, talcum powder, mica powder, heavy calcium carbonate, and microsilica powder, and the pigment is one or more of phthalocyanine pigment, iron oxide red, and titanium dioxide.

[0012] Preferably, the dispersant is one or more of modified polyacrylic acid polymer, controlled free radical polymerization acrylic acid block copolymer, and polyacrylic acid ammonium salt, and the defoamer is a mineral oil defoamer or a silicone polyether defoamer.

[0013] Preferably, the wetting and leveling agent is one or more of a hyperbranched polyether wetting agent, a modified polysiloxane, a fluorinated polyacrylate, and a modified siloxylate.

[0014] Preferably, the water-based additive is a porous resin and an oriented arrangement additive, and the anti-settling agent is one or more of bentonite, vinyl pyrrolidone copolymer, and modified urea.

[0015] Preferably, the decomposition functional material is a hydrophilic silicon-based porous material loaded with modified titanium dioxide, and the average particle size thereof is 0.1-20 μm.

[0016] Preferably, the modified titanium dioxide is one or more of N-Al-TiO2, N-Fe-TiO2, N-Pt-TiO2, and N-Ag-TiO2.

[0017] Preferably, the method for preparing the decomposition functional material comprises the following steps:

[0018] Step 1: Mix the silicon-based porous material with a particle size of 0.1-20 μm and the alkaline solution evenly, put them into a vacuum furnace and calcine them at 600-800° C. for 30±5 min, take them out to cool, grind and sieve them to obtain the silicon-based porous material with a particle size of 0.1-20 μm;

[0019] Step 2: titanate and ethanol are mixed at a molar mass ratio of 1:3.5-6, ammonium chloride and a soluble metal salt are mixed at a molar mass ratio of 1:1.1-1.5, and then dissolved in ethanol and water, acetic acid is used to adjust the pH to 3, and then dripped into the titanate ethanol solution and mixed evenly to form a gel;

[0020] Step 3: Add the silicon-based porous material obtained in step 1 to the gel obtained in step 2, soak for 10-20 minutes, filter out the filter cake, dry it, and then calcine it in a muffle furnace at 500-700°C for 2 hours, take it out, cool it, grind it, and sieve it to obtain a material with a particle size of 0.1-20 μm;

[0021] Step 4: hydrolyze the silane coupling agent containing -NH2 and -OH in a weak acid, add the material obtained in step 3 after hydrolysis until it turns blue, heat it in a water bath to 60-80°C and keep it warm for 2 hours, then filter it, dry the filter cake, heat it to 500-700°C under nitrogen protection and calcine it for 2 hours, take it out, cool, grind and sieve it to obtain a decomposition functional material with a particle size of 0.1-20μm.

[0022] Preferably, the titanate is one or more of tetrabutyl titanate and tetraethyl titanate, and the soluble metal salt is one or more of soluble salts of Fe, Al, Pt, and Ag.

[0023] The present invention also provides a method for preparing a two-component waterborne epoxy floor coating for degrading automobile exhaust as described in the above technical solution, comprising the following steps:

[0024] (1) Preparation of component A: Deionized water, dispersant, defoamer, pigment and filler are mixed and dispersed at high speed, and ground to a particle size of 5-20 μm, transferred to a dispersion tank, and decomposition functional materials are added and stirred at high speed for 20 minutes, and then water-based epoxy curing agent is added at low speed and stirred for 30 minutes. Wetting and leveling agent and anti-settling agent are added at low speed and stirred evenly, and then filtered to obtain component A;

[0025] (2) Preparation of component B: deionized water and water-based additives are added to the water-based epoxy emulsion under low-speed stirring to obtain component B;

[0026] (3) Component A and component B are mixed in proportion and stirred evenly to obtain a water-based epoxy floor coating that can degrade automobile exhaust.

[0027] Through the above technical scheme, it can be known that compared with the prior art, the present invention uses a hydrophilic silicon-based porous material loaded with modified titanium dioxide as a decomposition functional material, which has a higher specific surface area, so that the two-component water-based epoxy floor paint of the present invention has the ability to absorb solid suspended matter in automobile exhaust; the modified TiO2 enables the floor paint of the present invention to decompose CO, CH and nitrogen oxides in automobile exhaust under indoor visible light, and the effective removal rates of CO, CH and nitrogen oxides in the floor paint for 24 hours are 63.1%, 70.5% and 71.2% respectively. The present invention converts the paint film from hydrophilic to hydrophobic in the epoxy secondary dispersion film-forming process, so that the hydrophilic silicon-based porous material loaded with modified titanium dioxide moves to the surface of the paint film in a directional manner as the water evaporates during the film-forming process, effectively solving the problem that harmful gases cannot contact with the modified TiO2 caused by the film-forming on the surface of the floor paint, and the modified TiO2 is arranged on the surface layer to effectively improve the friction resistance of the coating. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The preparation process of the decomposition functional material is as follows:

[0030] Step 1: Mix the silicon-based porous material with a particle size of 0.1-20 μm and the alkaline solution evenly, put them into a vacuum furnace and calcine them at 600-800° C. for 30±5 min, take them out to cool, grind and sieve them to obtain the silicon-based porous material with a particle size of 0.1-20 μm;

[0031] Step 2: Tetrabutyl titanate and ethanol are mixed at a molar mass ratio of 1:4, ammonium chloride and ferric chloride are mixed at a molar mass ratio of 1:1.2, and then dissolved in ethanol and water, acetic acid is used to adjust the pH to 3, and then dripped into the titanate ethanol solution and mixed evenly to form a gel;

[0032] Step 3: Add the silicon-based porous material obtained in step 1 to the gel obtained in step 2, soak for 20 minutes, filter out the filter cake, dry it, and then calcine it in a muffle furnace at 630°C for 2 hours, take it out, cool it, grind it, and sieve it to obtain a material with a particle size of 0.1-20 μm;

[0033] Step 4: hydrolyze the KH550 silane coupling agent under weak acid, add the material obtained in step 3 after hydrolysis until it turns blue, heat to 80°C in a water bath and keep warm for 2 hours, filter, dry the filter cake, heat to 650°C under nitrogen protection and calcine for 2 hours, take out, cool, grind and sieve to obtain a decomposition functional material with a particle size of 0.1-20μm.

[0034] Example 1

[0035] The floor coating includes a curing agent component A and a water-based epoxy emulsion component B. The curing agent component A is composed of the following components in weight percentage: 32% deionized water, 35% water-based epoxy curing agent, 5% titanium dioxide, 10% barium sulfate, 10% microsilica powder, 0.8% dispersant, 0.2% defoaming agent, 0.8% wetting and leveling agent, 0.2% anti-settling agent and 5% decomposition material; the water-based epoxy emulsion component B is composed of the following components: 60% water-based epoxy emulsion, 38% deionized water, and 2% water-based additives; the ratio of components A to B is 2.5:1.

[0036] The preparation method of the floor coating comprises the preparation of components A and B.

[0037] Component A is prepared as follows: add 75kg of deionized water, 4kg of dispersant, 0.8kg of defoamer, 25kg of titanium dioxide, 50kg of barium sulfate, and 50kg of microsilica powder into a dispersion tank and disperse at high speed for 10 minutes, pour the white slurry into a grinder and grind it to a particle size of less than 20μm, take it out and put it into a dispersion tank, add 25kg of decomposition functional material and stir for 20 minutes at high speed, switch to low speed stirring, add 4kg of wetting and leveling agent, 85kg of deionized water, 175kg of water-based epoxy curing agent, and 1kg of magnesium aluminum silicate in sequence, stir for 30 minutes, filter, and discharge to obtain component A;

[0038] Component B: Add 120kg of water-based epoxy emulsion, 76kg of deionized water, and 4kg of water-based additive into a dispersion tank in sequence and disperse at low speed for 30 minutes, then filter to obtain component B;

[0039] Mix components A and B in a ratio of 2.5:1 and stir evenly to obtain a two-component water-based epoxy floor coating that can degrade automobile exhaust.

[0040] Example 2

[0041] The present invention discloses a two-component water-based epoxy floor coating capable of degrading automobile exhaust and an example of a preparation method thereof. The floor coating comprises an amide curing agent component A and a water-based epoxy emulsion component B, wherein the amide curing agent component A comprises the following components: 32% deionized water, 35% water-based epoxy curing agent, 5% titanium dioxide, 10% barium sulfate, 10% microsilica powder, 0.8% dispersant, 0.2% defoamer, 0.8% wetting and leveling agent, 0.2% anti-settling agent and 5% decomposition material; the water-based epoxy emulsion component B comprises the following components: 60% water-based epoxy emulsion, 38% deionized water and 2% water-based auxiliary agent; the ratio of components A to B is 2.5:1.

[0042] The preparation method of the floor coating comprises the preparation of components A and B. The preparation of component A is as follows: 75 kg of deionized water, 4 kg of dispersant, 0.8 kg of defoamer, 25 kg of titanium dioxide, 50 kg of barium sulfate, and 50 kg of microsilica powder are added to a dispersion tank for high-speed dispersion for 10 minutes, white slurry is poured into a grinder and ground to a particle size of less than 20 μm, taken out and put into a dispersion tank, 25 kg of decomposition functional material is added for high-speed stirring for 20 minutes, and then stirred at a low speed, 4 kg of wetting and leveling agent, 85 kg of deionized water, 175 kg of water-based epoxy curing agent, and 1 kg of magnesium aluminum silicate are added in sequence, and then stirred for 30 minutes, filtered, and discharged to obtain component A; for component B, 120 kg of water-based epoxy emulsion, 76 kg of deionized water, and 4 kg of water-based auxiliary agent are added to a dispersion tank in sequence for low-speed dispersion for 30 minutes, and filtered to obtain component B. Components A and B are mixed in a ratio of 2.5:1 and stirred evenly to obtain a two-component water-based epoxy floor coating capable of degrading automobile exhaust.

[0043] Example 3

[0044] The present invention discloses a two-component water-based epoxy floor coating capable of degrading automobile exhaust and an example of a preparation method thereof. The floor coating comprises an amide curing agent component A and a water-based epoxy emulsion component B. The amide curing agent component A comprises the following components: 32% deionized water, 35% water-based epoxy curing agent, 5% titanium dioxide, 8% barium sulfate, 9% microsilica powder, 0.8% dispersant, 0.2% defoamer, 0.8% wetting and leveling agent, 0.2% anti-settling agent and 8% decomposition material; the water-based epoxy emulsion component B comprises the following components: 60% water-based epoxy emulsion, 38% deionized water, and 2% water-based auxiliary agent; the ratio of components A to B is 2.5:1.

[0045] The preparation method of the floor coating comprises the preparation of components A and B. The preparation of component A is as follows: 75 kg of deionized water, 4 kg of dispersant, 0.8 kg of defoamer, 25 kg of titanium dioxide, 50 kg of barium sulfate, and 50 kg of microsilica powder are added to a dispersion tank for high-speed dispersion for 10 minutes, white slurry is poured into a grinder and ground to a particle size of less than 20 μm, taken out and put into a dispersion tank, 25 kg of decomposition functional material is added for high-speed stirring for 20 minutes, and then stirred at a low speed, 4 kg of wetting and leveling agent, 85 kg of deionized water, 175 kg of water-based epoxy curing agent, and 1 kg of magnesium aluminum silicate are added in sequence, and then stirred for 30 minutes, filtered, and discharged to obtain component A; for component B, 120 kg of water-based epoxy emulsion, 76 kg of deionized water, and 4 kg of water-based auxiliary agent are added to a dispersion tank in sequence for low-speed dispersion for 30 minutes, and filtered to obtain component B. Components A and B are mixed in a ratio of 2.5:1 and stirred evenly to obtain a two-component water-based epoxy floor coating capable of degrading automobile exhaust.

[0046] Test example

[0047] The test of removing harmful gases from automobiles in Examples 1-3 is as follows:

[0048] (1) CO gas is prepared by using oxalic acid and concentrated sulfuric acid, with a supersaturated lime water solution in the middle, and the gas is collected by the water displacement method; CH gas is simulated by using formaldehyde gas, taking a sealed iodine volumetric flask, placing formaldehyde solution in the flask, keeping it at a constant temperature of 28°C overnight, and extracting the upper gas, which is formaldehyde gas; NO gas is collected by the reaction of copper and dilute nitric acid by the water displacement method.

[0049] (2) Prepare floor paint samples on fiber-free cement boards in sequence, place the samples in a sealed glass box (no samples are placed in the blank group), connect the glass box to various harmful gas detectors (CO gas detector, formaldehyde gas detector, NO gas detector), install a fan in the glass box, and connect an air valve between the glass box and the harmful gas detector.

[0050] (3) Extract gas from the harmful gas collection bottle and inject it into the glass box, then seal the glass box. Turn on the fan to accelerate gas diffusion. Open the air valve, read and record the harmful gas value, and close the air valve. Read the value every 10 minutes, draw a time-harmful gas concentration graph, obtain the harmful gas degradation trend, and compare it with the blank group. Measure the purification rate after 24 hours.

[0051] The test results of the water-based floor paint on the purification effect of harmful gases for 24 hours are as follows:

[0052]

[0053] As can be seen from the above table, the concentrations of CO, formaldehyde, and NO in Example 1, Example 2, and Example 3 are significantly lower than those in the blank box. The purification rates of CO, formaldehyde, and NO in Example 1 for 24 hours are 62.1%, 65.7%, and 70%, respectively. The purification rates of CO, formaldehyde, and NO in Example 1 for 24 hours are 66.3%, 58%, and 63.4%, respectively. The purification rates of CO, formaldehyde, and NO in Example 1 for 24 hours are 63.1%, 70.5%, and 71.2%, respectively. This indicates that the water-based floor paint of the present invention has a good purification effect on CO, formaldehyde, and NO. Automobile exhaust mainly contains NO, CH, and CO, so the water-based floor paint of the present invention has an excellent purification function for automobile exhaust.

[0054] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0055] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust, characterized in that: Calculated by weight percentage, it includes the following components: Component A: deionized water 20-40%, water-based epoxy curing agent 30-50%, pigment and filler 20-50%, dispersant 0.1-1%, defoamer 0.1%-0.3%, wetting and leveling agent 0.1-1%, anti-settling agent 0.1-0.5%, decomposition functional material 3-10%; Component B: 50-80% water-based epoxy emulsion, 20-40% deionized water, 1-3% water-based additive; The weight ratio of the component A to the component B is 2.5:

1.

2. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 1, characterized in that: The filler in the color and filler is one or more of barium sulfate, rutile titanium dioxide, calcined kaolin, talc, mica powder, heavy calcium carbonate, and microsilica powder, and the pigment is one or more of phthalocyanine pigment, iron red, and titanium dioxide.

3. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 1, characterized in that: The dispersant is one or more of modified polyacrylic acid polymer, controlled free radical polymerization acrylic acid block copolymer, and polyacrylic acid ammonium salt; the defoamer is a mineral oil defoamer or an organosilicon polyether defoamer.

4. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 1, characterized in that: The wetting and leveling agent is one or more of a hyperbranched polyether wetting agent, a modified polysiloxane, a fluorinated polyacrylate, and a modified siloxylate.

5. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 1, characterized in that: The water-based additive is a porous resin and an alignment additive, and the anti-settling agent is one or more of bentonite, vinyl pyrrolidone copolymer, and modified urea.

6. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 1, characterized in that: The decomposition functional material is a hydrophilic silicon-based porous material loaded with modified titanium dioxide, and the average particle size thereof is 0.1-20 μm.

7. A two-component waterborne epoxy floor coating capable of degrading automobile exhaust according to claim 6, characterized in that: The modified titanium dioxide is one or more of N-Al-TiO2, N-Fe-TiO2, N-Pt-TiO2, and N-Ag-TiO2.

8. The two-component waterborne epoxy floor coating for degrading automobile exhaust according to claim 6, characterized in that: The preparation method of the decomposition functional material comprises the following steps: Step 1: Mix a silicon-based porous material with a particle size of 0.1-20 μm and an alkaline solution, place the mixture in a vacuum furnace and calcine it at 600-800°C for 30±5 minutes, take it out to cool, grind, and sieve to obtain a silicon-based porous material with a particle size of 0.1-20 μm; Step 2: titanate and ethanol are mixed at a molar mass ratio of 1:3.5-6, ammonium chloride and a soluble metal salt are mixed at a molar mass ratio of 1:1.1-1.5, and then dissolved in ethanol and water, and the pH is adjusted to 3 with acetic acid, and then the mixture is dropped into the titanate ethanol solution and mixed evenly to form a gel; Step 3: Add the silicon-based porous material obtained in step 1 to the gel obtained in step 2, soak for 10-20 minutes, filter out the filter cake, dry it, and then calcine it in a muffle furnace at 500-700°C for 2 hours, remove it, cool it, grind it, and sieve it to obtain a material with a particle size of 0.1-20 μm; Step 4: Hydrolyze the silane coupling agent containing -NH2 and -OH in a weak acid, add the material prepared in step 3 after hydrolysis until it turns blue, heat it to 60-80°C in a water bath and keep it warm for 2 hours, then filter it, dry the filter cake, heat it to 500-700°C under nitrogen protection and calcine it for 2 hours, take it out, cool it, grind it, and sieve it to obtain a decomposition functional material with a particle size of 0.1-20 μm.

9. The two-component waterborne epoxy floor coating for degrading automobile exhaust according to claim 8, characterized in that: The titanate is one or more of tetrabutyl titanate and tetraethyl titanate, and the soluble metal salt is one or more of soluble salts of Fe, Al, Pt, and Ag.

10. A method for preparing a two-component waterborne epoxy floor coating for degrading automobile exhaust according to claims 1-9, characterized in that: The following steps are involved: (1) Preparation of component A: Deionized water, dispersant, defoamer, pigment and filler are mixed and dispersed at high speed, and ground to a particle size of 5-20 μm. The mixture is transferred to a dispersion tank, and the decomposition functional material is added and stirred at high speed for 20 minutes. Then, the water-based epoxy curing agent is added at a low speed and stirred for 30 minutes. The wetting and leveling agent and anti-settling agent are added at a low speed and stirred evenly, and then filtered to obtain component A. (2) Preparation of component B: Deionized water and a water-based additive are added to the water-based epoxy emulsion under low-speed stirring to obtain component B; (3) Component A and component B are mixed in proportion and stirred evenly to obtain a water-based epoxy floor coating that can degrade automobile exhaust.

Citation Information

Patent Citations

  • Formaldehyde eliminating coating with dual functions of adsorption and decomposition and preparation method thereof

    CN103496884A

  • Water-borne floor paint capable of degrading formaldehyde

    CN105462445A

  • Preparation method and application of three-dimensional porous silicon carbon negative electrode material

    CN108550827A

  • Preparation method of Fe-N-TiO2 / 13X molecular sieve photocatalyst

    CN109759125A

  • Method for passivating acid sites on outer surface of L molecular sieve and application thereof