Corrosion-resistant self-cleaning surface treatment method for bathroom cabinet plate
By using micro-nano composites of silica and titanium dioxide and aminosilane coupling agents modified superhydrophobic functional fillers on the bathroom cabinet board, combined with epoxy resin to form a corrosion-resistant self-cleaning coating, the existing technology is solved. The surface treatment of bathroom cabinet boards is difficult to achieve superhydrophobic and self-cleaning problems, which significantly improves the resistance to mold corrosion and bactericidal ability.
Patent Information
- Application Number
- CN202411372793.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-29
AI Technical Summary
The surface treatment technology of existing bathroom cabinet wooden boards is difficult to achieve superhydrophobic and self-cleaning effects, and is susceptible to mold erosion, resulting in a reduced service life.
The nanostructures are prepared by hydrothermal method using micro-nano composites of silica and titanium dioxide, and modified with aminosilane coupling agent, ethyl chloroacetate and long-chain imidazole and other compounds to prepare superhydrophobic corrosion-resistant fillers. Physical blending is carried out in combination with epoxy resin and curing agent to form a corrosion-resistant self-cleaning coating.
It realizes superhydrophobicity and self-cleaning effect of the surface of the bathroom cabinet board, and has excellent killing ability to fight molds, significantly improving the resistance to mold corrosion.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface treatment, and in particular relates to a corrosion-resistant self-cleaning surface treatment method for a bathroom cabinet plate. Background Art
[0002] Bathroom cabinets refer to cabinets for placing items in bathrooms. They are made of various boards. Among them, the materials of existing boards (bathroom cabinet boards) can be roughly divided into several categories, such as wood, stone, metal, plastic, etc. Wood has gradually become the mainstream material of bathroom cabinet boards by virtue of its practicality, beauty, high strength and many other advantages. However, due to the common disadvantage of high water absorption of wood, it is often very easy to get damp during actual use, which leads to a large amount of erosion and corrosion by mold, greatly reducing the service life and practicality. Based on this, many existing technologies will choose to perform surface treatment on bathroom cabinet wood boards, such as lamination, to give it hydrophobic properties. However, these technologies still have certain disadvantages that limit their technical effects. This is because on the one hand, simple lamination treatment is difficult to achieve the super-hydrophobic nature of the surface, and it does not have the function of self-cleaning. On the other hand, the bathroom itself is an environment for the reproduction and growth of mold. Under the long-term joint action with moisture, the coating formed after lamination is also susceptible to erosion and destruction by mold, and ultimately cannot play the role it should have. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels. The present invention uses silicon dioxide as a micron-level structure, constructs nano-level titanium dioxide on its surface by a hydrothermal method, obtains a micro-nano composite, and then uses an aminosilane coupling agent as a modifier to modify the amino group, and then adds an ionic liquid containing carboxyl / long-chain alkane obtained by acidification through the action of ethyl chloroacetate and long-chain imidazole through halogen atoms and nitrogen, and a composite dehydroabietic acid, and the two are dehydrated and condensed with the amino group to prepare a super-hydrophobic corrosion-resistant functional filler. When the coating obtained by physically blending it with an epoxy resin and a curing agent at a relatively small addition amount is applied to the surface of a bathroom cabinet wooden board or an alloy board, the formed coating not only has a super-hydrophobic property and a self-cleaning effect, but also has an excellent killing ability against mold, and has very good mold corrosion resistance.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A method for treating a bathroom cabinet plate material with corrosion resistance and self-cleaning surface, the method comprising the following steps:
[0006] (1) coating the surface of the bathroom cabinet board with paint, drying, and forming a coating with a thickness of 0.2-0.25 mm, and the treatment is completed; the material of the bathroom cabinet board is wood or alloy; the coating comprises epoxy resin, curing agent and super hydrophobic corrosion resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the super hydrophobic corrosion resistant functional filler is 40-42:10-12:1.
[0007] As a preferred technical solution of the present invention, the method for preparing the coating in step (1) comprises the following steps:
[0008] Step X: Add the curing agent and the super-hydrophobic and corrosion-resistant functional filler into the epoxy resin, and then stir and mix at room temperature for 10-15 minutes to complete the preparation.
[0009] As a preferred technical solution of the present invention, the drying in step (1) refers to drying at a temperature of 60-70° C. for 8-10 hours.
[0010] As a preferred technical solution of the present invention, the curing agent in step (1) is diethylenetriamine.
[0011] As a preferred technical solution of the present invention, the super hydrophobic and corrosion-resistant functional filler in step (1) is prepared by the following steps:
[0012] Step A: adding glacial acetic acid to 40-50 parts by weight of an ethanol aqueous solution until the pH is adjusted to 2.5-3 to obtain a first solution; adding 0.1-0.15 parts by weight of silicon dioxide and 0.5-0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stirring and mixing at room temperature for 10-15 minutes to obtain a second solution; adding the second solution dropwise to the first solution while stirring, performing a hydrothermal reaction after the addition is completed, filtering, taking the filter residue, washing with deionized water, and then vacuum drying at 50-70° C. until constant weight, and finally heating to 500-520° C. at a heating rate of 4-6° C. / min, and then calcining at this temperature for 2 hours to obtain a micro-nano composite;
[0013] Step B: adding 0.1-0.2 parts by weight of deionized water, 1 part by weight of the micro-nano composite and 0.2-0.25 parts by weight of an aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stirring at 70-75° C. for 10-12 hours, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 50-70° C. until constant weight, to obtain an amino-modified micro-nano composite;
[0014] Step C: adding 5-6 parts by weight of long-chain imidazole to 6-7 parts by weight of ethyl chloroacetate, stirring at 60-65° C. for 24-26 hours, cooling naturally to room temperature, filtering, removing the filtrate, washing with ether, then adding 45-50 parts by weight of deionized water and 8-10 parts by weight of concentrated hydrochloric acid with a mass fraction of 35-38%, and finally stirring at 30-35° C. for 20-24 hours to remove impurities to obtain an ionic liquid;
[0015] Step D: Add 1-2 parts by weight of an amino-modified micro-nano composite, 0.3-0.4 parts by weight of an ionic liquid and 0.1-0.2 parts by weight of dehydroabietic acid to 60-80 parts by weight of anhydrous ethanol, and then stir and mix at room temperature for 5-10 minutes, adjust the pH to 3-3.5 with a hydrochloric acid solution, and then stir at 65-70° C. for 6-8 hours, filter, take the filter residue, wash it with anhydrous ethanol, and finally vacuum dry it at 50-70° C. until constant weight, and the preparation is completed.
[0016] Furthermore, the mass fraction of the ethanol aqueous solution in step A is 45-50%.
[0017] Furthermore, the particle size of the silicon dioxide in step A is 2-3 microns.
[0018] Furthermore, the dripping rate in step A is controlled at 1-2 drops / s.
[0019] Furthermore, the hydrothermal reaction in step A refers to heating the temperature in a hydrothermal reactor to 190-200° C. at a heating rate of 3-5° C. / min and then maintaining the temperature for 24 hours.
[0020] Furthermore, the aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
[0021] Furthermore, the long-chain imidazole in step C is at least one of 1-pentyl imidazole, N-n-hexyl imidazole and N-n-decyl imidazole.
[0022] Furthermore, the impurity removal in step C refers to distillation at 50° C. under a vacuum degree of -0.08 MPa until the volatiles are completely removed, followed by washing with ether, and finally vacuum drying at 40-45° C. until constant weight is reached.
[0023] Furthermore, the mass fraction of the hydrochloric acid solution in step D is 15-20%.
[0024] Beneficial effects of the present invention:
[0025] (1) The present invention uses silicon dioxide as a micron-sized structure, and constructs nano-sized titanium dioxide on its surface by a hydrothermal method to obtain a micro-nano composite, and then uses an aminosilane coupling agent as a modifier to modify the amino group, and then adds an ionic liquid containing carboxyl / long-chain alkane obtained by acidification through the action of ethyl chloroacetate and long-chain imidazole through halogen atoms and nitrogen, and a composite dehydroabietic acid, and the two are dehydrated and condensed with the amino group to prepare a super-hydrophobic and corrosion-resistant functional filler. When the coating obtained by physically blending it with an epoxy resin and a curing agent in a relatively small amount is applied to the surface of a bathroom cabinet wooden board or alloy board, the formed coating not only has a super-hydrophobic property and a self-cleaning effect, but also has an excellent killing ability against mold and has very good mold corrosion resistance.
[0026] (2) The present invention creatively combines micron-sized silicon dioxide and nano-sized titanium dioxide by a hydrothermal method to construct a micro-nano structure. On this basis, the amino modification of the silane coupling agent and the co-grafting of ionic liquid / dehydroabietic acid are carried out in sequence, and finally a super-hydrophobic and corrosion-resistant functional filler is prepared, which can achieve the super-hydrophobic property of the surface and excellent bactericidal ability with only a small amount of addition; the ionic liquid, as an imidazole salt compound, not only has a good bactericidal effect, but also its long-chain alkane structure can give the characteristic of low surface energy; dehydroabietic acid itself has many biological activities, such as antibacterial, and at the same time, from a structural point of view, one end group of it is also isopropyl, which has strong hydrophobicity. Therefore, after co-grafting with the ionic liquid, it can produce a certain synergistic effect and play an excellent role together.
[0027] (3) The surface treatment method provided by the present invention is universal and has excellent technical effects even for plates made of other materials, such as alloy plates, that is, it can give the surface super-hydrophobic properties and antibacterial properties. DETAILED DESCRIPTION
[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0029] The epoxy resins in all the embodiments and comparative examples of the present invention were purchased directly from the market, and were purchased from Hansen, with the model number EPIKOTE 6520-WH-53A; and the wood was all oak wood.
[0030] Example 1
[0031] A method for treating a bathroom cabinet plate material with corrosion resistance and self-cleaning surface, the method comprising the following steps:
[0032] (1) coating the surface of the bathroom cabinet board with paint, drying it to form a coating with a thickness of 0.2 mm, and the treatment is completed; the material of the bathroom cabinet board is wood; the coating comprises epoxy resin, curing agent and super hydrophobic corrosion resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the super hydrophobic corrosion resistant functional filler is 40:10:1.
[0033] The method for preparing the coating in step (1) comprises the following steps:
[0034] Step X: Add the curing agent and the super-hydrophobic and corrosion-resistant functional filler into the epoxy resin, and then stir and mix at room temperature for 10 minutes to complete the preparation.
[0035] The drying in step (1) refers to drying at a temperature of 60° C. for 8 hours.
[0036] The curing agent in step (1) is diethylenetriamine.
[0037] The super hydrophobic and corrosion resistant functional filler in step (1) is prepared by the following steps:
[0038] Step A: adding glacial acetic acid to 40 parts by weight of an ethanol aqueous solution until the pH is adjusted to 2.5 to obtain a first solution; adding 0.1 parts by weight of silicon dioxide and 0.5 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stirring and mixing at room temperature for 10 minutes to obtain a second solution; adding the second solution dropwise to the first solution while stirring, performing a hydrothermal reaction after the addition is completed, filtering, taking the filter residue, washing with deionized water, and then vacuum drying at 50° C. until constant weight, and finally heating to 500° C. at a heating rate of 4° C. / min and calcining at this temperature for 2 hours to obtain a micro-nano composite;
[0039] Step B: adding 0.1 parts by weight of deionized water, 1 part by weight of the micro-nano composite and 0.2 parts by weight of an aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stirring at 70° C. for 10 hours, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 50° C. until constant weight, to obtain an amino-modified micro-nano composite;
[0040] Step C: adding 5 parts by weight of long-chain imidazole to 6 parts by weight of ethyl chloroacetate, stirring at 60° C. for 24 hours, cooling naturally to room temperature, filtering, removing the filtrate, washing with ether, then adding 45 parts by weight of deionized water and 8 parts by weight of 35% concentrated hydrochloric acid, and finally stirring at 30° C. for 20 hours to remove impurities to obtain an ionic liquid;
[0041] Step D: Add 1 part by weight of an amino-modified micro-nano composite, 0.3 parts by weight of an ionic liquid and 0.1 parts by weight of dehydroabietic acid to 60 parts by weight of anhydrous ethanol, and then stir and mix at room temperature for 5 minutes, adjust the pH to 3 with a hydrochloric acid solution, then stir at 65°C for 6 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 50°C until constant weight, and the preparation is completed.
[0042] The mass fraction of the ethanol aqueous solution in step A is 45%.
[0043] The particle size of the silicon dioxide in step A is 2 microns.
[0044] The rate of dripping in step A is controlled at 1 drop / s.
[0045] The hydrothermal reaction in step A refers to heating the temperature in a hydrothermal reactor to 190° C. at a heating rate of 3° C. / min and then maintaining the temperature for 24 hours.
[0046] The aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
[0047] The long-chain imidazole in step C is N-n-decyl imidazole.
[0048] The impurity removal in step C refers to distillation at 50° C. under a vacuum degree of −0.08 MPa until the volatiles are completely removed, followed by washing with ether, and finally vacuum drying at 40° C. until constant weight.
[0049] The mass fraction of the hydrochloric acid solution in step D is 15%.
[0050] Example 2
[0051] A method for treating a bathroom cabinet plate material with corrosion resistance and self-cleaning surface, the method comprising the following steps:
[0052] (1) coating the surface of a bathroom cabinet board with paint, drying it, and forming a coating with a thickness of 0.25 mm, and the treatment is completed; the material of the bathroom cabinet board is wood; the coating comprises epoxy resin, a curing agent and a super-hydrophobic and corrosion-resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the super-hydrophobic and corrosion-resistant functional filler is 42:12:1.
[0053] The method for preparing the coating in step (1) comprises the following steps:
[0054] Step X: Add the curing agent and the super-hydrophobic and corrosion-resistant functional filler into the epoxy resin, and then stir and mix at room temperature for 15 minutes to complete the preparation.
[0055] The drying in step (1) refers to drying at a temperature of 70° C. for 10 hours.
[0056] The curing agent in step (1) is diethylenetriamine.
[0057] The super hydrophobic and corrosion resistant functional filler in step (1) is prepared by the following steps:
[0058] Step A: adding glacial acetic acid to 50 parts by weight of an ethanol aqueous solution until the pH is adjusted to 3 to obtain a first solution; adding 0.15 parts by weight of silicon dioxide and 0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stirring and mixing at room temperature for 15 minutes to obtain a second solution; adding the second solution dropwise to the first solution while stirring, performing a hydrothermal reaction after the addition is completed, filtering, taking the filter residue, washing with deionized water, and then vacuum drying at 70°C until constant weight, and finally heating to 520°C at a heating rate of 6°C / min and calcining at this temperature for 2 hours to obtain a micro-nano composite;
[0059] Step B: adding 0.2 parts by weight of deionized water, 1 part by weight of the micro-nano composite and 0.25 parts by weight of an aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stirring at 75° C. for 12 hours, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 70° C. until constant weight, to obtain an amino-modified micro-nano composite;
[0060] Step C: adding 6 parts by weight of long-chain imidazole to 7 parts by weight of ethyl chloroacetate, stirring at 65° C. for 26 hours, cooling naturally to room temperature, filtering, removing the filtrate, washing with ether, then adding 50 parts by weight of deionized water and 10 parts by weight of 38% concentrated hydrochloric acid, and finally stirring at 35° C. for 24 hours to remove impurities to obtain an ionic liquid;
[0061] Step D: Add 2 parts by weight of amino-modified micro-nano composite, 0.4 parts by weight of ionic liquid and 0.2 parts by weight of dehydroabietic acid to 80 parts by weight of anhydrous ethanol, and then stir and mix at room temperature for 10 minutes, adjust the pH to 3.5 with hydrochloric acid solution, then stir at 70°C for 8 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 70°C until constant weight, and the preparation is completed.
[0062] The mass fraction of the ethanol aqueous solution in step A is 50%.
[0063] The particle size of the silicon dioxide in step A is 3 microns.
[0064] The dripping rate in step A is controlled at 2 drops / s.
[0065] The hydrothermal reaction in step A refers to heating the temperature in a hydrothermal reactor to 200° C. at a heating rate of 5° C. / min and then maintaining the temperature for 24 hours.
[0066] The aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
[0067] The long-chain imidazole in step C is N-n-decyl imidazole.
[0068] The impurity removal in step C refers to distillation at 50° C. under a vacuum degree of −0.08 MPa until the volatiles are completely removed, followed by washing with ether, and finally vacuum drying at 45° C. until constant weight.
[0069] The mass fraction of the hydrochloric acid solution in step D is 20%.
[0070] Example 3
[0071] A method for treating a bathroom cabinet plate material with corrosion resistance and self-cleaning surface, the method comprising the following steps:
[0072] (1) coating the surface of a bathroom cabinet board with paint, drying it, and forming a coating with a thickness of 0.23 mm, and the treatment is completed; the material of the bathroom cabinet board is wood; the coating comprises epoxy resin, a curing agent and a super-hydrophobic and corrosion-resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the super-hydrophobic and corrosion-resistant functional filler is 41:11:1.
[0073] The method for preparing the coating in step (1) comprises the following steps:
[0074] Step X: Add the curing agent and the super-hydrophobic and corrosion-resistant functional filler into the epoxy resin, and then stir and mix at room temperature for 13 minutes to complete the preparation.
[0075] The drying in step (1) refers to drying at a temperature of 65° C. for 9 hours.
[0076] The curing agent in step (1) is diethylenetriamine.
[0077] The super hydrophobic and corrosion resistant functional filler in step (1) is prepared by the following steps:
[0078] Step A: adding glacial acetic acid to 45 parts by weight of an ethanol aqueous solution until the pH is adjusted to 2.8 to obtain a first solution; adding 0.13 parts by weight of silicon dioxide and 0.6 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stirring and mixing at room temperature for 13 minutes to obtain a second solution; adding the second solution dropwise to the first solution while stirring, performing a hydrothermal reaction after the addition is completed, filtering, taking the filter residue, washing with deionized water, and then vacuum drying at 60°C until constant weight, and finally heating to 510°C at a heating rate of 5°C / min and calcining at this temperature for 2 hours to obtain a micro-nano composite;
[0079] Step B: adding 0.15 parts by weight of deionized water, 1 part by weight of the micro-nano composite and 0.23 parts by weight of an aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stirring at 73° C. for 11 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 60° C. until constant weight, to obtain an amino-modified micro-nano composite;
[0080] Step C: adding 5.5 parts by weight of long-chain imidazole to 6.5 parts by weight of ethyl chloroacetate, stirring at 63° C. for 25 hours, cooling naturally to room temperature, filtering, removing the filtrate, washing with ether, then adding 48 parts by weight of deionized water and 9 parts by weight of 36% concentrated hydrochloric acid, and finally stirring at 33° C. for 22 hours to remove impurities to obtain an ionic liquid;
[0081] Step D: Add 1.5 parts by weight of an amino-modified micro-nano composite, 0.35 parts by weight of an ionic liquid and 0.15 parts by weight of dehydroabietic acid to 70 parts by weight of anhydrous ethanol, and then stir and mix at room temperature for 8 minutes, adjust the pH to 3.3 with a hydrochloric acid solution, then stir at 68°C for 7 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 60°C until constant weight, and the preparation is completed.
[0082] The mass fraction of the ethanol aqueous solution in step A is 48%.
[0083] The particle size of the silicon dioxide in step A is 3 microns.
[0084] The rate of the dripping in step A is controlled at 1.5 drops / s.
[0085] The hydrothermal reaction in step A refers to heating the temperature in a hydrothermal reactor to 195° C. at a heating rate of 4° C. / min and then maintaining the temperature for 24 hours.
[0086] The aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
[0087] The long-chain imidazole in step C is N-n-decyl imidazole.
[0088] The impurity removal in step C refers to distillation at 50° C. under a vacuum degree of −0.08 MPa until the volatiles are completely removed, followed by washing with ether, and finally vacuum drying at 43° C. until constant weight.
[0089] The mass fraction of the hydrochloric acid solution in step D is 18%.
[0090] Comparative Example 1
[0091] On the basis of Example 1, tetrabutyl titanate in step A was replaced by an equal weight of deionized water, and the rest remained unchanged.
[0092] Comparative Example 2
[0093] On the basis of Example 1, the ionic liquid in step D was changed to an equal weight of dehydroabietic acid, and the rest remained unchanged.
[0094] Comparative Example 3
[0095] On the basis of Example 1, the dehydroabietic acid in step D was replaced with an ionic liquid of equal weight, and the rest remained unchanged.
[0096] Test Example 1
[0097] Hydrophobic performance test:
[0098] The surface-treated bathroom cabinet plates of Examples 1-3 and Comparative Examples 1-3 were respectively subjected to static contact angle and rolling contact angle tests.
[0099] Table 1. Hydrophobicity test results
[0100] Static contact angle / ° Rolling contact angle / ° Example 1 156.2 6.0 Example 2 158.1 5.7 Example 3 156.4 5.9 Comparative Example 1 134.3 30.7 Comparative Example 2 144.4 16.9 Comparative Example 3 146.2 16.3
[0101] Test Example 2
[0102] Antibacterial performance test:
[0103] The surface-treated bathroom cabinet panels of Examples 1-3 and Comparative Examples 1-3 were respectively subjected to antibacterial performance tests (film pasting method) according to standard GB / T 21510-2008, and the tested fungus species was Aspergillus flavus.
[0104] Table 1. Antibacterial performance test results
[0105] Antibacterial rate / % Example 1 99.89 Example 2 99.90 Example 3 99.90 Comparative Example 1 99.87 Comparative Example 2 82.11 Comparative Example 3 87.52
[0106] From the comparison of test examples 1-2 and example 1 and comparative examples 1-3, it can be seen that after the surface treatment of the present invention, the obtained bathroom cabinet board not only has a super-hydrophobic property and a self-cleaning effect, but also has an excellent ability to kill mold and is very resistant to mold corrosion.
[0107] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels, characterized in that: The corrosion-resistant self-cleaning surface treatment method comprises the following steps: (1) coating the surface of the bathroom cabinet board with paint, drying, and forming a coating with a thickness of 0.2-0.25 mm, and the treatment is completed; the material of the bathroom cabinet board is wood or alloy; the coating comprises epoxy resin, curing agent and super hydrophobic corrosion resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the super hydrophobic corrosion resistant functional filler is 40-42:10-12:
1.
2. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 1, characterized in that: The method for preparing the coating in step (1) comprises the following steps: Step X: Add the curing agent and the super-hydrophobic and corrosion-resistant functional filler into the epoxy resin, and then stir and mix at room temperature for 10-15 minutes to complete the preparation.
3. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 1, characterized in that: The drying in step (1) refers to drying at a temperature of 60-70° C. for 8-10 hours.
4. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 1, characterized in that: The curing agent in step (1) is diethylenetriamine.
5. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 1, characterized in that: The super hydrophobic and corrosion resistant functional filler in step (1) is prepared by the following steps: Step A: adding glacial acetic acid to 40-50 parts by weight of an ethanol aqueous solution until the pH is adjusted to 2.5-3 to obtain a first solution; adding 0.1-0.15 parts by weight of silicon dioxide and 0.5-0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stirring and mixing at room temperature for 10-15 minutes to obtain a second solution; adding the second solution dropwise to the first solution while stirring, performing a hydrothermal reaction after the addition is completed, filtering, taking the filter residue, washing with deionized water, and then vacuum drying at 50-70° C. until constant weight, and finally heating to 500-520° C. at a heating rate of 4-6° C. / min, and then calcining at this temperature for 2 hours to obtain a micro-nano composite; Step B: adding 0.1-0.2 parts by weight of deionized water, 1 part by weight of the micro-nano composite and 0.2-0.25 parts by weight of an aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stirring at 70-75° C. for 10-12 hours, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 50-70° C. until constant weight, to obtain an amino-modified micro-nano composite; Step C: adding 5-6 parts by weight of long-chain imidazole to 6-7 parts by weight of ethyl chloroacetate, stirring at 60-65° C. for 24-26 hours, cooling naturally to room temperature, filtering, removing the filtrate, washing with ether, then adding 45-50 parts by weight of deionized water and 8-10 parts by weight of concentrated hydrochloric acid with a mass fraction of 35-38%, and finally stirring at 30-35° C. for 20-24 hours to remove impurities to obtain an ionic liquid; Step D: Add 1-2 parts by weight of an amino-modified micro-nano composite, 0.3-0.4 parts by weight of an ionic liquid and 0.1-0.2 parts by weight of dehydroabietic acid to 60-80 parts by weight of anhydrous ethanol, and then stir and mix at room temperature for 5-10 minutes, adjust the pH to 3-3.5 with a hydrochloric acid solution, and then stir at 65-70° C. for 6-8 hours, filter, take the filter residue, wash it with anhydrous ethanol, and finally vacuum dry it at 50-70° C. until constant weight, and the preparation is completed.
6. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 5, characterized in that: The particle size of the silicon dioxide in step A is 2-3 microns.
7. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 5, characterized in that: The hydrothermal reaction in step A refers to heating the temperature in a hydrothermal reactor to 190-200° C. at a heating rate of 3-5° C. / min and then maintaining the temperature for 24 hours.
8. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 5, characterized in that: The aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
9. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 5, characterized in that: The long-chain imidazole in step C is at least one of 1-pentyl imidazole, N-n-hexyl imidazole and N-n-decyl imidazole.
10. The corrosion-resistant self-cleaning surface treatment method for bathroom cabinet panels according to claim 5, characterized in that: The impurity removal in step C refers to distillation at 50° C. under a vacuum degree of -0.08 MPa until the volatiles are completely removed, followed by washing with ether, and finally vacuum drying at 40-45° C. until constant weight.
Citation Information
Patent Citations
Tensioning ground and rock anchoring bolt
EP0006520A1