Resistance-reducing sprayable organogel polymer surface coating for marine vehicles

CN119019930APending Publication Date: 2024-11-26SILVER FLAG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310598332.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The increase in fuel consumption and carbon emissions due to the increased shear resistance of marine transportation vehicles due to increased surface roughness. Existing drag reduction methods such as bubble technology consume high energy or use of toxic fluoride, and superhydrophobic coatings lack toughness and durability at high flow rates. sex.

Method used

Provides a sprayable polydimethylsiloxane (PDMS)-based organic gel polymer coating containing mineral oil and diluents, which creates a durable and smooth interface by spraying and curing, reducing ship resistance and possessing bioresistance. Pollution and corrosion resistance.

Benefits of technology

The coating significantly reduces water resistance, has high chemical and mechanical stability, is suitable for ships of different sizes and types, reduces fuel consumption and maintenance costs, and is environmentally and biologically harmless.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019930A_ABST
    Figure CN119019930A_ABST
Patent Text Reader

Abstract

The present application provides a drag reducing sprayable organogel polymer surface coating for marine vehicles. The coating is made of a coating material, and the coating material comprises a PDMS monomer and a curing agent; a diluent; and mineral oil. In the application of vehicles such as ships and the like, the coating disclosed by the invention has the remarkable beneficial effects in the aspects of drag reduction, durability, corrosion resistance, applicability, expansibility and the like, and has the advantages of being harmless and non-toxic to the environment and organisms in the environment, so that the coating disclosed by the invention has a great prospect in the application of the vehicles such as the ships and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of coating materials, in particular to coating materials for marine vehicles, and specifically relates to a drag-reducing sprayable organogel polymer (hereinafter referred to as "SOP") surface coating for ships. Background Art

[0002] Marine vehicles require strength and energy to resist drag, so during cruising, marine vehicles consume fuel and emit carbon dioxide (CO2) into the atmosphere. For a typical container or transport ship, more than 50% of the drag is caused by shear drag on the hull. [1] , while for slow-speed transport vessels this fraction may be 80–90% [2] . Shear drag therefore accounts for a large portion of fuel consumption and carbon emissions. International shipping accounts for 3% of global CO2 emissions [3] , 765 million tons of carbon dioxide were emitted in 2020 [4] The situation can be even worse when surface roughness is increased due to biofouling or corrosion. Drag can increase by up to 190% compared to a surface without biofouling. [5] In addition to the added drag of biofouling, removal of biofouling also requires significant expenditures, accounting for 10% to 20% of total operating costs. Costs range from $200,000 to $500,000, depending on container size, and represent approximately 20-50% of a tanker’s annual revenue. [6] Therefore, there is a need to investigate feasible, scalable, and durable coatings for marine vehicles to alleviate these two issues.

[0003] There are two main methods on the market to solve the drag problem. One of them is to use bubbles. Bubbles are released under the ship, acting as a buffer layer between the ship and the water, thereby reducing drag. However, this method requires up to 10% of the total energy consumption of marine vehicles. [7] Therefore, the energy savings vary and the final energy consumption may be higher after applying this method. Another method is to use coating application on ships, which uses fluorinated chemicals [8] Or super hydrophobic coating [9] However, both coatings have their limitations: fluoride is banned in many countries due to its inherent toxicity to the ocean and marine life, while superhydrophobic surfaces lack toughness and durability under high flow rates.

[10] Therefore, there is still a need to develop an effective and non-toxic coating for marine vehicles to effectively solve the above problems. Summary of the invention

[0004] Technical Purpose

[0005] In view of the above problems, the technical purpose of the present invention is to provide a fully functional, scalable and durable sprayable coating composition.

[0006] Another technical purpose of the present invention is to provide a coating prepared from the above coating composition. The coating is suitable for ships and vehicles of different sizes and types, can give ships and vehicles a chemically and mechanically stable smooth interface, and provide them with drag reduction, anti-biological fouling and anti-corrosion properties, while having the advantages of harmlessness, durability and scale adjustability, thereby reducing fuel consumption and maintenance costs of marine vehicles.

[0007] Another technical object of the present invention is to provide a method for preparing the above coating from the above coating composition.

[0008] Another technical object of the present invention is to provide an article comprising a substrate and the above-mentioned coating on the surface of the substrate.

[0009] Another technical purpose of the present invention is to provide a method for reducing ship resistance.

[0010] Technical content

[0011] In order to solve the above technical problems, on the one hand, the present invention provides a coating material, which comprises:

[0012] PDMS monomer and curing agent, wherein the weight ratio of PDMS monomer to curing agent is about 15-5:1;

[0013] a diluent having a weight ratio of about 2 to 0.5:1 to the total weight of the PDMS monomer and the curing agent; and

[0014] The mineral oil is contained in an amount of about 10-15% based on 100 parts by weight of the total weight of the coating material.

[0015] In some embodiments, the PDMS monomer is a dimethylsiloxane oligomer.

[0016] In some embodiments, the curing agent may be a Pt catalyst. In some embodiments, the weight ratio of PDMS monomer to curing agent is about 15 to 5:1, such as about 15:1, 13:1, 12:1, 11:1, 10:1, 9:1, 8:1, 7:1, 5:1, etc., preferably about 10:1.

[0017] In some embodiments, the PDMS monomer and curing agent may be SYLGARD from Dow Corning. TM 184. SYLGARD TM184 is a two-component composition, component A is a PDMS monomer, and component B is a curing agent. When used, component A and component B are used in a weight ratio of about 10:1.

[0018] The mineral oil, also known as white oil, has a CAS number of 8042-47-5.

[0019] In some embodiments, the diluent is selected from n-hexane and toluene.

[0020] In some embodiments, the weight ratio of the diluent to the total weight of the PDMS monomer and the curing agent is about 2 to 0.5:1, for example, about 2:1, 1.5:1, 1.3:1, 1.1:1, 1:1, 0.9:1, 0.8:1, 0.7:1, 0.5:1, etc., preferably about 1:1.

[0021] In some embodiments, the mineral oil content is about 10-15%, such as about 10%, 11%, 12%, 13%, 14%, 15%, etc., based on 100 parts by weight of the total weight of the coating material, preferably about 13%.

[0022] In another aspect, the present invention provides a method for preparing a coating using the above coating material, the method comprising the following steps:

[0023] 1) Mixing PDMS monomer and curing agent in proportion to form a pre-curing mixture;

[0024] 2) adding a diluent to the pre-cured mixture to obtain a diluted mixture;

[0025] 3) adding mineral oil to the diluted mixture obtained in step 2) to obtain a coating;

[0026] 4) applying the coating obtained in step 3) to a substrate; and

[0027] 5) Curing the coating applied to the substrate in step 4) to obtain the coating.

[0028] In some embodiments, steps 1)-3) are all performed at room temperature.

[0029] In some embodiments, in step 2), n-hexane or toluene is added as a diluent, wherein the weight ratio of the pre-cured mixture to the diluent may be about 2 to 0.5:1, preferably about 1:1.

[0030] There is no particular limitation on the mixing method in steps 1)-3), as long as the mixture can be mixed evenly. In some embodiments, the mixing can be performed by stirring. For example, the mixture can be stirred at about 1000 rpm for about 5 minutes, but is not limited thereto.

[0031] In some embodiments, in step 4), the substrate may be any surface that requires drag reduction, corrosion resistance, chemical durability, mechanical durability, hydrophobicity, and / or slippery properties. In some embodiments, the substrate may be made of a conductive or non-conductive material, including metals such as steel (including stainless steel, carbon steel, iron, etc.), aluminum, copper, or polymers such as plastics, acrylonitrile butadiene styrene (ABS), wood, paper, ceramics, or other materials, but not limited thereto.

[0032] In some embodiments, in step 4), the application is carried out by spraying, for example, by using a spray gun or other similar device to spray the coating onto the substrate. Preferably, the coating is sprayed onto the substrate at a pressure of about 2 to 4 bars.

[0033] In some embodiments, in step 5), the coating can be cured at a temperature of about 150° C. at room temperature. For example, the coating can be cured at room temperature or heated to about 80 to 150° C. At room temperature, the curing time is about 2 days. In the case of heating, the curing time can be shortened to about 10 minutes to about 3 hours depending on the temperature of the heating.

[0034] In another aspect, the present invention provides a coating comprising a PDMS polymer matrix and mineral oil uniformly dispersed in the PDMS polymer matrix.

[0035] In some embodiments, the coating has a thickness of about 10-50 μm, for example, about 10, 20, 25, 30, 40, 45, 50 μm, etc., preferably about 20-50 μm.

[0036] In some embodiments, the coating is prepared using the coating material according to the present invention or using the method for preparing a coating using the coating material according to the present invention.

[0037] In yet another aspect, the present invention provides an article comprising a substrate and the above-mentioned coating on a surface of the substrate.

[0038] The substrate can be made of conductive or non-conductive materials, including but not limited to metals such as steel (including stainless steel, carbon steel, iron, etc.), aluminum, copper, etc., polymers such as plastic, acrylonitrile butadiene styrene (ABS), etc., wood, paper, ceramics or other materials.

[0039] The coatings and substrates described herein may be present on one or more surfaces of a variety of different types of articles. The exact use environment of the article may vary, and the exact configuration of the article may vary.

[0040] In some embodiments, the substrate of the article is in direct contact with the coating.

[0041] In some embodiments, the substrate may include surface features or textures. The surface features or textures may be produced by etching the substrate.

[0042] The product includes but is not limited to pipes, bathroom equipment, and transportation vehicles. In some embodiments, the product is selected from water pipelines, canals, water culverts, bathroom equipment, and transportation vehicles. Preferably, the product is a transportation vehicle.

[0043] In still another aspect, the present invention provides a transportation vehicle having a surface in contact with water, wherein the surface has the above-mentioned coating.

[0044] In some embodiments, the means of transport are not particularly limited, in particular, means of transport on or in water, which may include vehicles, ships, aircraft, etc., among which ships are preferred, such as rowboats, sailboats, container ships, cruise ships, cruise ships, oil tankers, natural gas tankers, polar ships, fishing boats, warships, aircraft carriers, cruisers, battleships, torpedo boats, destroyers, anti-submarine boats, submarines, semi-submarine boats, cargo ships, passenger ships, barges, etc., but are not limited thereto.

[0045] In some embodiments, all surfaces of the transport vehicle in contact with water have the above coating. In other embodiments, only part of the surface of the transport vehicle in contact with water has the above coating.

[0046] In yet another aspect, the present invention provides a vessel comprising a vessel body and the above coating on a surface of the vessel body in contact with water.

[0047] The vessel is not particularly limited and may be any surface or underwater vessel, such as rowboats, sailboats, container ships, cruise ships, cruise liners, oil tankers, gas tankers, polar ships, fishing vessels, warships, aircraft carriers, cruisers, battleships, torpedo boats, destroyers, submarine hunters, submarines, semi-submersible ships, cargo ships, passenger ships, barges, etc., but are not limited thereto.

[0048] In some embodiments, all surfaces of the ship in contact with water have the coating. In other embodiments, only part of the surface of the ship in contact with water has the coating.

[0049] In yet another aspect, the present invention provides a method for reducing resistance of a ship, the method comprising the step of forming the above coating on a surface of the ship in contact with water.

[0050] The vessel is not particularly limited and may be any surface or underwater vessel, such as rowboats, sailboats, container ships, cruise ships, cruise liners, oil tankers, gas tankers, polar ships, fishing vessels, warships, aircraft carriers, cruisers, battleships, torpedo boats, destroyers, submarine hunters, submarines, semi-submersible ships, cargo ships, passenger ships, barges, etc., but are not limited thereto.

[0051] In some embodiments, the coating is formed on all surfaces of the ship in contact with water. In other embodiments, the coating is formed on a portion of the surface of the ship in contact with water.

[0052] The method for forming the above coating on the surface of the ship in contact with water is consistent with the method for forming the above coating described above, and will not be repeated here.

[0053] Beneficial Effects

[0054] In summary, the SOP surface coating of the present invention is a novel, cost-effective and scalable coating that can reduce water resistance while having high chemical and mechanical stability. The coating uses polydimethylsiloxane as the base material because it has excellent mechanical properties, making the coating durable. In addition, PDMS is an organic gel that can absorb oils and has strong cohesion with them, which helps to form a stable and smooth interface on the substrate.

[0055] Specifically, the advantages of the coating of the present invention are embodied in the following points:

[0056] 1). The coating of the present invention has significant drag reduction performance under different Reynolds numbers. Tests show that the coating of the present invention can reduce drag by 40% at low Re and by at least 7% at high Re.

[0057] 2). The coating of the present invention is durable and can maintain the drag reduction, wettability and smoothness of the surface for a long time.

[0058] 3). The coating of the present invention also has strong corrosion resistance.

[0059] 4). The coating of the present invention has applicability and scalability, and is suitable for ships of different sizes / shapes.

[0060] 5) The coating of the present invention is a mixture of chemical materials and oil. Since the materials constituting the coating are absolutely harmless to the environment and human body, the coating also naturally has the advantages of being harmless and non-toxic to the environment and the organisms in the environment.

[0061] 6) The coating of the present invention has the advantage of strong operability. By using the oily composite mixture, the coating material is sprayed on a transportation vehicle, such as a ship, and then hardened and dried with a hot air gun, or allowed to harden naturally, a very durable and strong coating can be obtained, thus having the advantage of simple operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 : Schematic diagram of the SOP surface coating preparation process.

[0063] Figure 2: (a) Contact angle and (b) hysteresis angle measurements.

[0064] Figure 3 : Drag reduction percentage at different Reynolds numbers.

[0065] Figure 4 : Durability test results of coated aluminum panels.

[0066] Figure 5 : Relationship between cruising speed and power input for coated and uncoated remote controlled boats.

[0067] Figure 6 : Contact angle and hysteresis angle after sandpaper friction.

[0068] Figure 7 : Weight measured during acid corrosion test.

[0069] Figure 8 : Contact angle and hysteresis angle of the coating after immersion in seawater. DETAILED DESCRIPTION

[0070] Hereinafter, the technical solution of the present application is described in detail through specific implementation modes so that those skilled in the art can better understand the present invention; however, these implementation modes are not intended to limit the scope of the present invention.

[0071] The composition, preparation process and performance evaluation of the coating of the present application are described in detail below through specific examples.

[0072] the term

[0073] Herein, the sprayable organogel polymer is referred to as "SOP (Sprayable organogel polymer)".

[0074] Unless otherwise stated, the numerical values ​​in the present invention represent approximate measurements or limitations of the range of embodiments including minor deviations from given values ​​and having approximately the mentioned values ​​and having the mentioned exact values. Except for the last example described in detail, all numerical values ​​of parameters (e.g., quantities or conditions) in this application document (including the appended claims) should be understood as modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value described allows for slight imprecision (some close to precision in the value; approximately or reasonably close to the value; approximately). If the imprecision provided by "about" is not understood in this ordinary sense in the art, the "about" used herein at least represents the changes that can be produced by ordinary methods of measuring and using these parameters. For example, "about" can include less than or equal to 15%, less than or equal to 10%, less than or equal to 5%, less than or equal to 4%, less than or equal to 3%, less than or equal to 2%, less than or equal to 1%, less than or equal to 0.5%, less than or equal to 0.1% change, and in some aspects, less than or equal to 0.01% change.

[0075] Preparation Example 1: Preparation of coating

[0076] The coating comprising a PDMS polymer matrix and mineral oil was prepared as Figure 1 As shown in the figure, PDMS monomer and curing agent used are Dow Corning's SYLGARD TM 184. First, SYLGARD, a PDMS monomer, TM Component A (silicon elastomer) of 184 and SYLGARD as curing agent TM Component B (curing agent) of 184 was mixed in a weight ratio of 10:1 to form a pre-cured mixture Premix 1. The pre-cured mixture Premix 1 was mixed at 1000 rpm for 5 minutes, and then n-hexane (CAS: 110-54-3, RCI Labscan) was added as a diluent in a weight ratio of 1:1 to obtain a mixture Premix 2. Mineral oil (CAS: 8042-47-5, Sigma-Aldrich) was then added to Premix 2 (the mineral oil content was 13% based on the total weight of the coating material) and stirred at 1000 rpm for another 5 minutes. The coating was then sprayed onto an aluminum substrate using a spray gun at a pressure of 2 to 4 bars, with a coating thickness of 10 to 50 μm. The coating was then placed at room temperature (25°C) or heated to 80 to 150°C to accelerate the curing process. At room temperature, the curing time was 2 days, which could be shortened to 3 hours to 10 minutes depending on the heating temperature. After the coating was cured, the SOP surface coating was manufactured.

[0077] Test Example 1: Contact Angle and Hysteresis Angle Measurement

[0078] In this example, the contact angle and hysteresis angle of the coating were measured. The images were taken with a high-magnification camera and then analyzed with a graphics program (Image J).

[0079] The experimental results are as follows Figure 2 As shown, from Figure 2 It can be seen that the SOP surface coating according to the present application has strong hydrophobicity (contact angle of about 111°) and low adhesion of water droplets.

[0080] Test Example 2: Drag reduction performance evaluation in a water tunnel

[0081] The shear stress of the surface can be obtained by measuring the pressure drop when water flows over the surface. Water tunnels providing various Reynolds numbers (Re) ranging from 4000 to 23500 were built to test the drag reduction performance of the coating. The pressure difference before and after the surface was measured to obtain the shear resistance. The aluminum substrate coated with the SOP surface coating prepared according to Preparation Example 1 (coating thickness of about 20 μm) was compared with an aluminum plate not coated with the coating to obtain the drag reduction percentage.

[0082] The results are as follows Figure 3 As shown. Figure 3 It can be seen that the drag reduction can reach 40% at low Re, while the drag reduction is at least 7% at high Re.

[0083] Test Example 3: Drag Reduction Sustainability Evaluation

[0084] In addition to drag reduction performance, the sustainability of drag reduction is also an important criterion for the feasibility of the coating. The aluminum substrate coated with the SOP surface coating prepared according to Preparation Example 1 was tested continuously for 48 hours at the highest Re, and the drag reduction percentage was measured every 2 hours. The results are shown in Figure 2. Figure 4 shown.

[0085] In other studies, the highest durability of drag reduction was only 16 hours [11-13] , and Re is less than 600, therefore, Figure 4 It is shown that the SOP surface coating of the present application can continuously reduce drag at Re of about 23,500, which indicates that the SOP surface coating of the present application has a durable drag reduction performance.

[0086] Test Example 4: Evaluation of drag reduction performance of remote-controlled boat

[0087] The speed of a remote-controlled boat made of acrylonitrile butadiene styrene (ABS) was measured before and after coating with a SOP surface coating according to the present application (coating method see Preparation Example 1). The remote-controlled boat was tested in a lake, and a GPS speedometer was placed inside the hull to measure the cruising speed. The relationship between cruising speed and power input is shown in Figure 5 shown.

[0088] from Figure 5 It can be seen that for the same power input, the speed of the remote control boat can be increased by at least 6%, and the maximum increase can reach 22%. Taking into account the resistance of the ship, the maximum reduction is 18% and the minimum is 6%.

[0089] Test Example 5: Evaluation of Mechanical Durability of Coating

[0090] The aluminum substrate coated with the SOP surface coating prepared according to Preparation Example 1 was rubbed with sandpaper to test the mechanical durability of the coating. The mechanical durability of the coating of marine vehicles is important because floating objects may be encountered during cruising. A strong coating is preferred because it helps to provide sustainable performance.

[0091] In this test example, the SOP surface coating prepared in Preparation Example 1 was treated with 1600-grit sandpaper and a normal pressure of 1 kPa. The contact angle and hysteresis angle after every 10 frictions (a total of 100 frictions) were plotted on Figure 6 middle.

[0092] from Figure 6 It can be seen that the SOP surface coating according to the present application is mechanically stable, and the wettability and smoothness of the coating are not significantly changed by friction.

[0093] Test Example 6: Evaluation of the Corrosion Resistance of Coating

[0094] Chemical stability is important for marine vehicle coatings because rainwater and seawater are weakly acidic and can corrode the hull and change the wettability of the coating. In this test example, an aluminum substrate coated with the SOP surface coating prepared in Preparation Example 1 and an aluminum substrate not coated with the coating were placed in 2M hydrochloric acid to test the anti-corrosion performance. The weight was measured throughout the experiment, and the results are shown in Figure 7 shown.

[0095] from Figure 7 It can be seen that the aluminum substrate coated with the SOP surface coating according to the present application has no significant weight change after being treated with acid, while the aluminum substrate without the coating has a significant weight loss. The results show that the coating helps prevent corrosion.

[0096] In addition, the aluminum substrate coated with the SOP surface coating prepared according to Preparation Example 1 was placed under seawater to examine the changes in wettability and smoothness due to seawater corrosion. The aluminum substrate coated with the SOP surface coating was immersed in seawater for 5 weeks, and the contact angle and hysteresis angle were measured every week. The results are shown in Figure 8 middle.

[0097] Figure 8 The results showed that there was no significant change in the hysteresis angle and the contact angle.

[0098] In summary, the above Figure 7 and 8 The results show that the SOP surface coating of the present application is chemically stable.

[0099] From the results of the above test embodiments, it can be seen that the SOP surface coating of the present application has significant beneficial effects in terms of drag reduction, durability, corrosion resistance, applicability, and expansibility, and has the advantages of being harmless and non-toxic to the environment and organisms in the environment. Therefore, the SOP surface coating of the present application has great prospects in the application of ships and other means of transportation.

[0100] References:

[0101] [1]M.Perlin, Mitigation of Hydrodynamic Resistance, WORLD SCIENTIFIC, 2015.

[0102] [2]AGElkafas,MMElgohary,AEZeid,Alexandria Engineering Journal2019,58,849.

[0103] [3]Future Ship Powering Options Exploring Alternative Methods of ShipPropulsion, 2013.

[0104] [4]CM,GD,SE,MM,SE,M.-FF,BM,OJ,GG,RS,VE,GHG Emissions ofAll World Countries,Publications Office Of The European Union,Luxembourg(Luxembourg),2021.

[0105] [5]MP Schultz, GWSwain, Biofouling 2000,15,129.

[0106] [6]A.Apostolidis,A.Merikas,A.Merika,The Journal of ComputationalOptimization in Economics and Finance 2013,5,27.

[0107] [7]I.Kumagai,Y.Takahashi,Y.Murai,Ocean Engineering 2015,95,183.

[0108] [8]G.Luo,L.Wen,K.Yang,X.Li,S.Xu,P.Pi,X.Wen,Chemical EngineeringJournal 2020,383,123125.

[0109] [9]RJDaniello,NEWaterhouse,JPRothstein,Physics of Fluids 2009,21,085103.

[0110]

[10] E.Aljallis,MASarshar,R.Datla,V.Sikka,A.Jones,C.-H.Choi,Physicsof Fluids 2013,25,025103.

[0111]

[11] H.Yan,F.Qian,K.Jiao,W.Zhang,Z.Tan,L.Zhao,Q.Wang,C.Zhao,MicrofluidNanofluidics 2022,26,77.

[0112]

[12] J.-H.Kim,JPRothstein,Exp Fluids 2016,57,81.

[0113]

[13] MASamaha,HVTafreshi,M.Gad-el-Hak,Langmuir 2012,28,9759.

Claims

1. A coating material comprising: PDMS monomer and curing agent, wherein the weight ratio of PDMS monomer to curing agent is 15 to 5:1; A diluent, wherein the weight ratio of the diluent to the total weight of the PDMS monomer and the curing agent is 2 to 0.5:1; and The mineral oil is contained in an amount of 10-15% based on 100 parts by weight of the total weight of the coating material.

2. The coating material according to claim 1, wherein The PDMS monomer is a dimethylsiloxane oligomer.

3. The coating material according to claim 1, wherein The curing agent is a Pt catalyst.

4. The coating material according to claim 1, wherein The weight ratio of PDMS monomer to curing agent is 10:

1.

5. The coating material according to claim 1, wherein The PDMS monomer and curing agent are SYLGARD from Dow Corning TM 184.

6. The coating material according to claim 1, wherein The weight ratio of the diluent to the total weight of the PDMS monomer and the curing agent is 1:

1.

7. The coating material according to claim 1, wherein The diluent is selected from n-hexane and toluene.

8. The coating material according to claim 1, wherein The mineral oil content is 13%, based on 100 parts by weight of the total weight of the coating material.

9. A method for preparing a coating using the coating material according to any one of claims 1 to 8, the method comprising the following steps: 1) Mixing PDMS monomer and curing agent in proportion to form a pre-curing mixture; 2) adding a diluent to the pre-cured mixture to obtain a diluted mixture; 3) adding mineral oil to the diluted mixture obtained in step 2) to obtain a coating; 4) applying the coating obtained in step 3) to a substrate; as well as 5) Curing the coating applied to the substrate in step 4) to obtain the coating.

10. The method according to claim 9, wherein: In step 4), the substrate is any surface requiring drag reduction, corrosion resistance, chemical durability, mechanical durability, hydrophobicity and / or slippery properties.

11. The method according to claim 9, wherein: In step 4), the substrate is made of metal, polymer, wood, paper or ceramic.

12. The method according to claim 9, wherein: In step 4), the application is carried out by spraying.

13. The method according to claim 9, wherein: In step 5), the coating is cured at room temperature or heated to 80 to 150°C.

14. A coating comprising a PDMS polymer matrix and mineral oil uniformly dispersed in the PDMS polymer matrix.

15. The coating according to claim 14, wherein The coating has a thickness of 10-50 μm.

16. The coating according to claim 14, wherein The coating is prepared using the coating material according to any one of claims 1 to 8 or by the method according to any one of claims 9 to 13.

17. An article comprising a substrate and a coating according to any one of claims 14 to 16 on a surface of the substrate.

18. A transportation vehicle, comprising a surface in contact with water, wherein the surface comprises the coating according to any one of claims 14 to 16.

19. The transport vehicle according to claim 18, wherein: The transport means is a ship.

20. A ship comprising a ship hull and a coating according to any one of claims 14 to 16 on a surface of the ship hull in contact with water.

21. A method for reducing resistance of a ship, the method comprising the step of forming the coating according to any one of claims 14 to 16 on a surface of the ship in contact with water.