High-toughness PET adhesive tape and preparation method thereof

By introducing conductive fillers and modification technologies into PET tape, the problems of electrostatic and dust adsorption of traditional tapes are solved, the anti-static and conductive properties are improved, and the functional needs of miniaturization and diversification of electronic products are met.

CN119019948AInactive Publication Date: 2024-11-26DONGGUAN SOGO IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410720714.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional tape is prone to static electricity and dust adsorption in electronic products, affecting heat dissipation and service life, and cannot meet the functional needs brought about by the miniaturization and diversification of electronic products.

Method used

PET substrate is used as the tape matrix, and the surface is coated with pressure-sensitive adhesive. The conductive filler is introduced into the pressure-sensitive adhesive to form composite particles through graphene oxide and silica nanoparticles, and modified by silane coupling agent and quaternary ammonium grafting. Improve conductivity and anti-static ability.

Benefits of technology

High toughness PET tape was prepared, which has excellent anti-static properties and conductivity, reduces dielectric losses, enhances dispersion and compatibility in the organism, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-toughness PET adhesive tape and a preparation method thereof, the high-toughness PET adhesive tape comprises a PET base material, the surface of one side of the PET base material is coated with a pressure-sensitive adhesive, and a release film is adhered to the pressure-sensitive adhesive; the pressure-sensitive adhesive is prepared from the following raw materials in parts by weight: 80 to 95 parts of acrylate-based adhesive, 10 to 15 parts of conductive filler, 10 to 15 parts of diluent, 1 to 1.5 parts of accelerant and 0.1 to 0.3 part of flatting agent; according to the antistatic adhesive tape, the PET material is used as a matrix, the adhesive tape is endowed with high toughness through the excellent toughness of the PET material, the pressure-sensitive adhesive is adhered, the pressure-sensitive adhesive takes acrylate as a matrix, and the pressure-sensitive adhesive can be endowed with excellent conductivity and improved antistatic capacity by introducing the conductive filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive tapes, and in particular to a high-toughness PET tape and a preparation method thereof. Background Art

[0002] PET, or polyethylene terephthalate, is made by exchanging dimethyl terephthalate with ethylene glycol or by esterifying terephthalic acid with ethylene glycol to synthesize dihydroxyethyl terephthalate, and then subjecting it to a condensation reaction. The toughness of the film made from it is the best among all thermoplastics, and its tensile strength and impact strength are much higher than those of ordinary films. It also has good strength and dimensional stability. It also has excellent heat resistance, cold resistance, good chemical resistance and oil resistance, and is widely used in the base tape of insulating tape.

[0003] However, with the development of electronic technology, the use of tape in the electronic industry is also expanding. With the development of the diversity of electronic products and the miniaturization of electronic products, new requirements have been put forward for the function of tape. In electronic products, traditional tapes are prone to static electricity, and the static electricity on the surface of the tape is easy to absorb dust, which will affect the heat dissipation and service life of electronic products. Therefore, antistatic tapes have emerged. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a high-toughness PET tape and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A high-toughness PET tape comprises a PET substrate, one side of the PET substrate is coated with a pressure-sensitive adhesive, and the pressure-sensitive adhesive is adhered to a release film; The pressure-sensitive adhesive comprises the following raw materials in parts by weight: 80-95 parts of acrylate base glue, 10-15 parts of conductive filler, 10-15 parts of diluent, 1-1.5 parts of accelerator, and 0.1-0.3 parts of leveling agent; The conductive filler is prepared by the following steps: Step S1, adding graphene oxide and polyvinyl pyrrolidone prepared by Hummer's method to 80% ethanol aqueous solution, ultrasonically dispersing for 1h, then dropping 10% ammonia water to adjust the pH until the system pH = 9, slowly dropping tetraethyl orthosilicate, stirring at a constant speed for 12h at room temperature after the addition, filtering after the stirring, washing the filter cake three times with deionized water to obtain composite particles, and controlling the amount ratio of graphene oxide, polyvinyl pyrrolidone and tetraethyl orthosilicate to be 0.1-0.2g: 0.1-0.2g: 0.1-0.15mL; In step S1, tetraethyl orthosilicate is used as a silicon source to in-situ hydrothermally generate silica nanoparticles on the surface of graphene oxide to obtain graphene oxide-loaded silica nanoparticles. The introduced nano-silicon dioxide can provide more deep traps to inhibit the migration of carriers, thereby maintaining low dielectric loss and conductive properties of the composite particles.

[0006] Step S2, adding N,N-dimethylethanolamine to acetone, adding allyl chloride dropwise, heating to 40°C, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying to obtain a quaternary ammonium salt, wherein the molar ratio of allyl chloride to N,N-dimethylethanolamine is controlled to be 1-1.2:1; In step S2, N,N-dimethylethanolamine and allyl chloride react to form a quaternary ammonium salt, and a carbon-carbon double bond and an alcoholic hydroxyl group are introduced into the structure; Step S3, adding the composite particles and KH570 into a 10% by volume ethanol aqueous solution, heating to 40-45° C., stirring at a constant speed and reacting for 4 hours, and obtaining grafted composite particles after the reaction is completed; In step S3, the surface of the composite particles is modified by a silane coupling agent KH570, and the hydroxyl groups formed by the hydrolysis of KH570 are condensed with the hydroxyl groups on the surface of the composite particles, thereby connecting the carbon-carbon double bonds on the surface of KH570 to the surface of the composite particles to obtain grafted composite particles, and the weight ratio of the composite particles to KH570 is controlled to be 1-1.2:1.5-2.

[0007] Step S4, adding the grafted composite particles and maleic anhydride into deionized water, adding a 30% by mass aqueous hydrogen peroxide solution, introducing nitrogen to expel oxygen, dropping a 10% by mass aqueous ferrous chloride solution, raising the temperature to 35-40° C., and keeping the temperature for reaction for 5 hours. After the reaction is completed, the modified composite particles are obtained, and the weight ratio of the grafted composite particles, maleic anhydride, the hydrogen peroxide solution and the ferrous chloride solution is controlled to be 10:1-2:0.1-0.2:0.1-0.2; In step S4, the carbon-carbon double bonds on the grafted composite particles are polymerized with the carbon-carbon double bonds on the maleic anhydride, and are hydrolyzed to form carboxyl groups; Step S5, adding the prepared modified composite particles and the quaternary ammonium salt prepared in step S2 into deionized water, stirring at a uniform speed and adding p-toluenesulfonic acid hydrate, heating to 80-85°C, stirring at a uniform speed and reacting for 24 hours to obtain conductive particles, and controlling the weight ratio of the modified composite particles, the quaternary ammonium salt and the p-toluenesulfonic acid hydrate to be 10:2-3:0.2-0.3.

[0008] In step S5, the carboxyl groups on the modified composite particles and the hydroxyl groups on the quaternary ammonium salt structure undergo esterification reaction under the action of the catalyst p-toluenesulfonic acid hydrate, and then the quaternary ammonium salt structure is grafted on the surface of the composite particles. By grafting the polymer on the surface of the composite particles, on the one hand, the dispersibility of the composite particles in the organism can be improved to prevent agglomeration. On the other hand, the quaternary ammonium salt introduced with the cation can cooperate with the composite particles to exert excellent conductive properties and play an antistatic effect. In addition, the carbon-carbon double bond structure is introduced on the quaternary ammonium salt, which can be better compatible with the acrylic resin organism. Finally, by making a polymer grafted on the surface of the composite particles, the problem of the quaternary ammonium salt itself being easy to migrate in the organism as a small molecule can also be prevented.

[0009] Furthermore, the diluent is allyl glycidyl ether.

[0010] Furthermore, the accelerator is polyetheramine.

[0011] Furthermore, the pressure-sensitive adhesive is prepared by the following steps: The acrylate-based adhesive and the diluent are mixed, and then the conductive filler, the accelerator and the leveling agent are added in sequence and mixed evenly, and vacuum degassing is performed to obtain the pressure-sensitive adhesive.

[0012] A method for preparing a high-toughness PET tape comprises the following steps: The surface of one side of the PET base film is corona treated and then coated with a pressure-sensitive adhesive, and then a release film is adhered to the release film through the pressure-sensitive adhesive to obtain a high-toughness PET tape.

[0013] The beneficial effects of the present invention are as follows: the present invention prepares a PET tape, which uses PET material as a matrix, and gives the tape high toughness through the excellent toughness of the PET material itself, and adheres a pressure-sensitive adhesive, the pressure-sensitive adhesive uses acrylate as a matrix, and can give the pressure-sensitive adhesive excellent electrical conductivity and improve antistatic ability by introducing a conductive filler. In the preparation process of the conductive filler, ethyl orthosilicate is used as a silicon source, and silicon dioxide nanoparticles are hydrothermally generated in situ on the surface of graphene oxide to obtain graphene oxide-loaded silicon dioxide nanoparticles, and composite particles are prepared. The introduced nano-silicon dioxide can provide more deep traps to inhibit the migration of carriers, so that the composite particles maintain low dielectric loss and conductive performance, and the surface of the composite particles is modified by a silane coupling agent KH570, thereby K The carbon-carbon double bonds on the surface of H570 are connected to the surface of the composite particles, and then polymerized with the carbon-carbon double bonds on maleic anhydride to prepare modified composite particles. Finally, the carboxyl groups on the modified composite particles and the hydroxyl groups on the quaternary ammonium salt structure undergo an esterification reaction under the action of a catalyst, p-toluenesulfonic acid hydrate, and then the quaternary ammonium salt structure is grafted on the surface of the composite particles. By grafting the polymer on the surface of the composite particles, on the one hand, the dispersibility of the composite particles in the organism can be improved to prevent agglomeration. On the other hand, the quaternary ammonium salt with the introduction of cations can cooperate with the composite particles to exert excellent conductive properties and have an antistatic effect. In addition, the carbon-carbon double bond structure introduced on the quaternary ammonium salt can be better compatible with the acrylic resin organism. Finally, by making a polymer grafted on the surface of the composite particles, the problem of the quaternary ammonium salt itself being a small molecule and easily migrating in the organism can be prevented. DETAILED DESCRIPTION

[0014] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0015] A high-toughness PET tape comprises a PET substrate, one side of the PET substrate is coated with a pressure-sensitive adhesive, and the pressure-sensitive adhesive is adhered to a release film; A method for preparing a high-toughness PET tape comprises the following steps: The surface of one side of the PET base film is corona treated and then coated with a pressure-sensitive adhesive, and then a release film is adhered to the release film through the pressure-sensitive adhesive to obtain a high-toughness PET tape.

[0016] The pressure-sensitive adhesive comprises the following raw materials in parts by weight: 80 parts of acrylic base glue, 10 parts of conductive filler, 10 parts of diluent, 1 part of accelerator, and 0.1 part of leveling agent; The pressure-sensitive adhesive is prepared by the following steps: The acrylate-based adhesive and the diluent are mixed, and then the conductive filler, the accelerator and the leveling agent are added in sequence and mixed evenly, and vacuum degassing is performed to obtain the pressure-sensitive adhesive.

[0017] The diluent is allyl glycidyl ether.

[0018] The accelerator is polyetheramine.

[0019] The conductive filler is prepared by the following steps: Step S1, adding graphene oxide and polyvinyl pyrrolidone prepared by Hummer's method to 80% ethanol aqueous solution, ultrasonically dispersing for 1h, then dropping 10% ammonia water to adjust the pH until the system pH = 9, slowly dropping tetraethyl orthosilicate, stirring at a constant speed for 12h at room temperature after the dropping, filtering after the stirring, washing the filter cake three times with deionized water to obtain composite particles, and controlling the amount ratio of graphene oxide, polyvinyl pyrrolidone and tetraethyl orthosilicate to be 0.1g:0.1g:0.1mL; Step S2, adding N,N-dimethylethanolamine to acetone, adding allyl chloride dropwise, heating to 40°C, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying to obtain a quaternary ammonium salt, wherein the molar ratio of allyl chloride to N,N-dimethylethanolamine is controlled to be 1:1; Step S3, adding the composite particles and KH570 into a 10% by volume ethanol aqueous solution, heating to 40° C., stirring at a constant speed and reacting for 4 hours, and obtaining grafted composite particles after the reaction is completed; Step S4, adding the grafted composite particles and maleic anhydride into deionized water, adding a 30% by mass aqueous hydrogen peroxide solution, introducing nitrogen to expel oxygen, dropping a 10% by mass aqueous ferrous chloride solution, raising the temperature to 35° C., and keeping the temperature for reaction for 5 hours. After the reaction is completed, the modified composite particles are obtained, and the weight ratio of the grafted composite particles, maleic anhydride, the hydrogen peroxide solution and the ferrous chloride solution is controlled to be 10:1:0.1:0.1; Step S5, adding the prepared modified composite particles and the quaternary ammonium salt prepared in step S2 into deionized water, stirring at a uniform speed and adding p-toluenesulfonic acid hydrate, heating to 80°C, stirring at a uniform speed and reacting for 24 hours to obtain conductive particles, and controlling the weight ratio of the modified composite particles, the quaternary ammonium salt and the p-toluenesulfonic acid hydrate to be 10:2:0.2. Example

[0020] A high-toughness PET tape comprises a PET substrate, one side of the PET substrate is coated with a pressure-sensitive adhesive, and the pressure-sensitive adhesive is adhered to a release film; A method for preparing a high-toughness PET tape comprises the following steps: The surface of one side of the PET base film is corona treated and then coated with a pressure-sensitive adhesive, and then a release film is adhered to the release film through the pressure-sensitive adhesive to obtain a high-toughness PET tape.

[0021] The pressure-sensitive adhesive comprises the following raw materials in parts by weight: 90 parts of acrylic base glue, 12 parts of conductive filler, 12 parts of diluent, 1.3 parts of accelerator, and 0.2 parts of leveling agent; The pressure-sensitive adhesive is prepared by the following steps: The acrylate-based adhesive and the diluent are mixed, and then the conductive filler, the accelerator and the leveling agent are added in sequence and mixed evenly, and vacuum degassing is performed to obtain the pressure-sensitive adhesive.

[0022] The diluent is allyl glycidyl ether.

[0023] The accelerator is polyetheramine.

[0024] The conductive filler is prepared by the following steps: Step S1, adding graphene oxide and polyvinyl pyrrolidone prepared by Hummer's method to 80% ethanol aqueous solution, ultrasonically dispersing for 1h, then dropping 10% ammonia water to adjust the pH until the system pH = 9, slowly dropping tetraethyl orthosilicate, stirring at a constant speed for 12h at room temperature after the addition, filtering after the stirring, washing the filter cake three times with deionized water to obtain composite particles, and controlling the amount ratio of graphene oxide, polyvinyl pyrrolidone and tetraethyl orthosilicate to be 0.2g:0.2g:0.12mL; Step S2, adding N,N-dimethylethanolamine to acetone, adding allyl chloride dropwise, heating to 40°C, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying to obtain a quaternary ammonium salt, wherein the molar ratio of allyl chloride to N,N-dimethylethanolamine is controlled to be 1.1:1; Step S3, adding the composite particles and KH570 into a 10% by volume ethanol aqueous solution, heating to 44° C., stirring at a constant speed and reacting for 4 hours, and obtaining grafted composite particles after the reaction is completed; Step S4, adding the grafted composite particles and maleic anhydride into deionized water, adding a 30% by mass aqueous hydrogen peroxide solution, introducing nitrogen to expel oxygen, dropping a 10% by mass aqueous ferrous chloride solution, raising the temperature to 38° C., and keeping the temperature for reaction for 5 hours. After the reaction is completed, the modified composite particles are obtained, and the weight ratio of the grafted composite particles, maleic anhydride, the hydrogen peroxide solution and the ferrous chloride solution is controlled to be 10:1.5:0.1:0.2; Step S5, adding the prepared modified composite particles and the quaternary ammonium salt prepared in step S2 into deionized water, stirring at a uniform speed and adding p-toluenesulfonic acid hydrate, heating to 82°C, stirring at a uniform speed and reacting for 24 hours to obtain conductive particles, and controlling the weight ratio of the modified composite particles, the quaternary ammonium salt and the p-toluenesulfonic acid hydrate to be 10:2.5:0.3. Example

[0025] A high-toughness PET tape comprises a PET substrate, one side of the PET substrate is coated with a pressure-sensitive adhesive, and the pressure-sensitive adhesive is adhered to a release film; A method for preparing a high-toughness PET tape comprises the following steps: The surface of one side of the PET base film is corona treated and then coated with a pressure-sensitive adhesive, and then a release film is adhered to the release film through the pressure-sensitive adhesive to obtain a high-toughness PET tape.

[0026] The pressure-sensitive adhesive comprises the following raw materials in parts by weight: 95 parts of acrylate base glue, 15 parts of conductive filler, 15 parts of diluent, 1.5 parts of accelerator, and 0.3 parts of leveling agent; The pressure-sensitive adhesive is prepared by the following steps: The acrylate-based adhesive and the diluent are mixed, and then the conductive filler, the accelerator and the leveling agent are added in sequence and mixed evenly, and vacuum degassing is performed to obtain the pressure-sensitive adhesive.

[0027] The diluent is allyl glycidyl ether.

[0028] The accelerator is polyetheramine.

[0029] The conductive filler is prepared by the following steps: Step S1, adding graphene oxide and polyvinyl pyrrolidone prepared by Hummer's method to 80% ethanol aqueous solution, ultrasonically dispersing for 1h, then dropping 10% ammonia water to adjust the pH until the system pH = 9, slowly dropping tetraethyl orthosilicate, stirring at a constant speed for 12h at room temperature after the addition, filtering after the stirring, washing the filter cake three times with deionized water to obtain composite particles, and controlling the amount ratio of graphene oxide, polyvinyl pyrrolidone and tetraethyl orthosilicate to be 0.2g:0.2g:0.15mL; Step S2, adding N,N-dimethylethanolamine to acetone, adding allyl chloride dropwise, heating to 40°C, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying to obtain a quaternary ammonium salt, wherein the molar ratio of allyl chloride to N,N-dimethylethanolamine is controlled to be 1.2:1; Step S3, adding the composite particles and KH570 into a 10% by volume ethanol aqueous solution, heating to 45° C., stirring at a constant speed and reacting for 4 hours, and obtaining grafted composite particles after the reaction is completed; Step S4, adding the grafted composite particles and maleic anhydride into deionized water, adding a 30% by mass aqueous hydrogen peroxide solution, introducing nitrogen to expel oxygen, dropping a 10% by mass aqueous ferrous chloride solution, raising the temperature to 40° C., and keeping the temperature for reaction for 5 hours. After the reaction is completed, the modified composite particles are obtained, and the weight ratio of the grafted composite particles, maleic anhydride, the hydrogen peroxide solution and the ferrous chloride solution is controlled to be 10:2:0.2:0.2; Step S5, adding the prepared modified composite particles and the quaternary ammonium salt prepared in step S2 into deionized water, stirring at a uniform speed and adding p-toluenesulfonic acid hydrate, heating to 85°C, stirring at a uniform speed and reacting for 24 hours to obtain conductive particles, and controlling the weight ratio of the modified composite particles, the quaternary ammonium salt and the p-toluenesulfonic acid hydrate to be 10:3:0.3.

[0030] Comparative Example 1 Compared with Example 3, this comparative example uses the composite particles prepared in step S1 as the conductive filler, and the rest is the same as Example 3.

[0031] Comparative Example 2 Compared with Example 3, this comparative example uses nano-silicon dioxide instead of composite particles, and the rest is the same as Example 3.

[0032] The properties of the adhesive tapes prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in Table 1 below: A comma blade was used to coat a 25 μm thick adhesive layer on the surface of a 25 μm PET substrate, and the layers were aged at 55°C for 2 days. The antistatic value, peel strength and initial adhesion performance were tested.

[0033] Table 1

[0034] It can be seen from Table 1 above that the adhesive tapes prepared in Examples 1-3 of the present invention have excellent antistatic properties, and the conductive filler has little effect on the bonding properties of the pressure-sensitive adhesive.

[0035] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A high-toughness PET tape, characterized in that: It comprises a PET substrate, one side of the PET substrate is coated with a pressure-sensitive adhesive, and the pressure-sensitive adhesive is adhered with a release film; The pressure-sensitive adhesive comprises the following raw materials in parts by weight: 80-95 parts of acrylate base glue, 10-15 parts of conductive filler, 10-15 parts of diluent, 1-1.5 parts of accelerator, and 0.1-0.3 parts of leveling agent; The conductive filler is prepared by the following steps: Step S1, adding graphene oxide and polyvinyl pyrrolidone prepared by Hummer's method to an ethanol aqueous solution with a volume fraction of 80%, ultrasonically dispersing for 1 hour, then dripping 10% ammonia water to adjust the pH until the system pH is 9, slowly dripping ethyl orthosilicate, stirring at a constant speed for 12 hours at room temperature after the dripping, filtering after the stirring, and washing the filter cake with deionized water three times to obtain composite particles; Step S2, adding N,N-dimethylethanolamine to acetone, adding allyl chloride dropwise, heating to 40°C, stirring at a constant speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying to obtain a quaternary ammonium salt; Step S3, adding the composite particles and KH570 into a 10% by volume ethanol aqueous solution, heating to 40-45° C., stirring at a constant speed and reacting for 4 hours, and obtaining grafted composite particles after the reaction is completed; Step S4, adding the grafted composite particles and maleic anhydride into deionized water, adding a 30% by mass aqueous hydrogen peroxide solution, introducing nitrogen to expel oxygen, dripping a 10% by mass aqueous ferrous chloride solution, raising the temperature to 35-40° C., keeping the temperature for reaction for 5 hours, and obtaining modified composite particles after the reaction is completed; Step S5, adding the prepared modified composite particles and the quaternary ammonium salt prepared in step S2 into deionized water, stirring at a uniform speed and adding p-toluenesulfonic acid hydrate, heating to 80-85° C., stirring at a uniform speed and reacting for 24 hours to prepare conductive particles.

2. A high-toughness PET tape according to claim 1, characterized in that: The diluent is allyl glycidyl ether.

3. A high-toughness PET tape according to claim 1, characterized in that: The accelerator is polyetheramine.

4. A high-toughness PET tape according to claim 1, characterized in that: In step S1, the amount ratio of graphene oxide, polyvinyl pyrrolidone and tetraethyl orthosilicate is controlled to be 0.1-0.2g: 0.1-0.2g: 0.1-0.15mL, the molar ratio of allyl chloride and N, N-dimethylethanolamine is controlled to be 1-1.2: 1 in step S2, the weight ratio of composite particles and KH570 is controlled to be 1-1.2: 1.5-2 in step S3, the weight ratio of grafted composite particles, maleic anhydride, aqueous hydrogen peroxide solution and aqueous ferrous chloride solution is controlled to be 10: 1-2: 0.1-0.2: 0.1-0.2 in step S4, and the weight ratio of modified composite particles, quaternary ammonium salt and p-toluenesulfonic acid hydrate is controlled to be 10: 2-3: 0.2-0.3 in step S5.

5. A high-toughness PET tape according to claim 1, characterized in that: The pressure-sensitive adhesive is prepared by the following steps: The acrylate-based adhesive and the diluent are mixed, and then the conductive filler, the accelerator and the leveling agent are added in sequence and mixed evenly, and vacuum degassing is performed to obtain the pressure-sensitive adhesive.

6. The method for preparing a high-toughness PET tape according to claim 1, characterized in that: The steps include: The surface of one side of the PET base film is corona treated and then coated with a pressure-sensitive adhesive, and then a release film is adhered to the release film through the pressure-sensitive adhesive to obtain a high-toughness PET tape.

Citation Information

Patent Citations

  • Flame-retardant antistatic protective film and preparation method thereof

    CN113528041A